Method for recovering ultra-fine particle titanium concentrate from vanadium-titanium magnetite concentrate upgrading tailings
Through the process of weak magnetization iron removal, strong magnetic separation and flotation desulfurization and titanium selection in vanadium titanium magnet concentrate quality improvement tailings, combined with the chemical adjustment, the problem of difficult recovery of ilmenite crystals is solved, and the problem of improvement of ilmenite crystals has been improved. Titanium concentrate grade and recovery rate.
Patent Information
- Application Number
- CN202411393749.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-06
AI Technical Summary
The existing technology is difficult to effectively recover vanadium titanium magnet concentrate quality-enhancing tailings, especially ilmenite, which is finely ground from iron concentrate. The monomer dissociation degree is low, making it difficult to recover. , the existing process is difficult to improve the grade and recovery rate of titanium concentrate.
After weak magnetization is used to remove iron, strong magnetic coarse selection and strong magnetic sweep selection are carried out, combined with cyclone concentration, flotation desulfurization and titanium selection, and adjust the agent system and process parameters, including H2SO4, yellow medicine, 2# oil and capture The dosage of agent is selected several times to improve the grade and recovery of titanium concentrate.
The dissociation of each particle level in iron concentrate quality-improved tailings was improved, titanium loss was reduced, and efficient recovery of titanium concentrate was achieved. The TiO2 grade was increased to 46.00-49.32%, and the recovery rate reached 75%-85%.
Smart Images

Figure CN119076202A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a method for recovering ultrafine titanium concentrate from tailings obtained by upgrading vanadium-titanium magnetite concentrate. Background Art
[0002] At present, the tailings of vanadium-titanium magnetite concentrate in Panxi area can obtain TiO by the combined process of "strong magnetic separation + flotation". 2 For titanium concentrate with a grade of about 47%, this process has a good recovery effect for ilmenite with a particle size of +38um, but the recovery effect for ilmenite with a particle size of -38um is not ideal, and efficient utilization of resources cannot be achieved.
[0003] The loss of fine ilmenite can be roughly divided into four categories: (1) the inclined plate overflow produced by the concentration of iron ore tailings; (2) the fine ilmenite that enters the strong magnetic tailings during the strong magnetic tailings discarding process; (3) the inclined plate overflow produced by the inclined plate before flotation; (4) the ultra-fine ilmenite of the tailings of iron ore upgrading. Among them, the fine ilmenite of types (1), (2) and (3) is the fine ilmenite produced by the over-grinding of ilmenite during the iron and titanium selection process. Its monomer dissociation degree is relatively high, and the monomer dissociation degree gradually increases as the particle size becomes finer. The fourth type of fine-grained ilmenite is ilmenite guest crystal finely ground from iron ore concentrate, and its monomer dissociation degree gradually decreases as the particle size becomes finer. Therefore, the theoretical flotation grade of the fourth type of fine-grained ilmenite is lower than that of the first, second and third type of fine-grained ilmenite, and its comprehensive recovery is more difficult. The existing recovery process for the first, second and third type of fine-grained ilmenite is difficult to effectively recover the fourth type of fine-grained ilmenite.
[0004] CN115301400A discloses a method for beneficiating ultrafine ilmenite, which comprises the following steps: S1, strong magnetic roughing: subjecting the ultrafine ilmenite to strong magnetic roughing at a magnetic field strength of 0.8-1.2T to obtain a magnetic concentrate and a magnetic tailing; S2, strong magnetic scavenging: subjecting the magnetic tailing to strong magnetic scavenging at a magnetic field strength of 1.1-1.5T to obtain a magnetic concentrate and a magnetic tailing; S3, combining and concentrating the magnetic concentrate and the magnetic concentrate to obtain a floating material; S4, subjecting the floating material to one or more roughing, five or more concentrating, and one or more scavenging steps to obtain a titanium concentrate; the roughing, concentrating and scavenging methods all adopt flotation method; the ultrafine ilmenite ore: TiO 2 The grade of is 13-18%, the grade of TFe is 14-19%; -0.018mm content accounts for 75-85%, TiO 2 The distribution rate is 80-90%.
[0005] CN112871437A discloses a method for recovering ultrafine ilmenite, which comprises the following steps: S1. performing strong magnetic separation on the raw ore to obtain floating material and magnetic separation tailings; S2. performing rough separation on the floating material using a flotation column to obtain a rougher concentrate and a rougher tailings; S3. performing primary titanium concentration and secondary titanium concentration on the rougher concentrate in sequence to obtain a titanium concentrate; wherein the primary titanium concentration adopts a flotation column, and the secondary concentration adopts a flotation machine; the raw ore is an ultrafine ilmenite with a mass percentage of minerals with a particle size of -0.019 mm greater than 70%.
[0006] However, the above method is still for the beneficiation of fine-grained ilmenite of types (1), (2) and (3) with good selectivity, and is difficult to be applied to fine-grained ilmenite of type (4). Summary of the invention
[0007] In view of the problems of the prior art, the purpose of the present invention is to develop a method for recovering ultrafine titanium concentrate from the tailings of vanadium-titanium magnetite concentrate to increase the concentrate grade and recovery rate.
[0008] To achieve the above object, the present invention provides a method for recovering ultrafine titanium concentrate from the upgraded tailings of vanadium-titanium magnetite concentrate, which comprises the following steps:
[0009] A. Perform weak magnetic iron removal on the iron concentrate upgrading tailings with a magnetic field strength of 3000Gs to obtain iron concentrate and iron tailings;
[0010] B. The iron tailings obtained in step A are subjected to strong magnetic roughing. In the strong magnetic roughing, the diameter of the magnetic medium is 1.5 mm, the magnetic field strength is 1.2 T, the pulsation stroke is 2.5 CM, and the pulsation stroke is 300 times / min to obtain strong magnetic roughing concentrate and strong magnetic roughing tailings;
[0011] The strong magnetic roughing tailings are subjected to strong magnetic sweeping, in which the diameter of the concentrated magnetic medium is 2 mm, the magnetic field strength is 0.9 T, the pulsation stroke is 3 CM, and the pulsation frequency is 300 times / min, to obtain strong magnetic sweeping concentrate and strong magnetic sweeping tailings; the strong magnetic roughing concentrate and the strong magnetic sweeping concentrate are combined as strong magnetic concentrate;
[0012] C. Concentrating the strong magnetic concentrate obtained in step B by a cyclone to obtain cyclone sedimentation and cyclone overflow, and controlling the mass concentration of cyclone sedimentation to be 40% to 50%;
[0013] D. flotation desulfurization of the cyclone sediment obtained in step C to obtain desulfurized tailings and crude cobalt sulfide ore;
[0014] E. The desulfurization tailings obtained in step D are subjected to flotation separation to select titanium to obtain titanium concentrate and titanium-selected tailings.
[0015] Among them, the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step A, the TiO 2 The grade is 12-13.46%, and the -19μm content is 55-78%.
[0016] Among them, the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step B, the TiO 2 The grade is 18.56~22.54%.
[0017] Among them, in the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step D, the flotation desulfurization process is one roughing and two sweeping.
[0018] Among them, in the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step D, in flotation desulfurization, the amount of desulfurization roughing agent used is: H 2 SO 4 800~1000g / t cyclone sand settling, 150~180g / t xanthate cyclone sand settling, 20~30g / t 2# oil cyclone sand settling.
[0019] Among them, in the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step E, the flotation process of titanium separation is one coarse, three fine and one sweep.
[0020] Among them, in the above-mentioned method for efficiently recovering ultrafine ilmenite in the quality-improving tailings, in step E, in the flotation titanium selection, the reagent system for the flotation titanium roughing selection is: 2 SO 4 The dosage is 2000-2600g / t desulfurization tailings, the dosage of the adjusting agent is 200-400g / t desulfurization tailings, the dosage of the collecting agent is 2400-2800g / t desulfurization tailings, the dosage of the diesel is 500-700g / t desulfurization tailings, and the adjusting agent is composed of water glass, sodium tripolyphosphate and ethylenediaminetetraacetic acid (the proportion is the conventional proportion in this field).
[0021] Among them, in the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step E, the specific operation of flotation titanium selection is: subjecting the desulfurized tailings obtained in step D to flotation titanium roughing to obtain a rough titanium concentrate and a roughing tailing; subjecting the rough titanium concentrate to a first selection, and using H before the first selection 2 SO 4 Adjust the pH of the slurry to 3.4-3.6 to obtain concentrate 1 and concentrate 1 tailings; conduct the second concentration of concentrate 1, and use H 2 SO 4 Adjust the pH of the slurry to 3.1-3.3 to obtain concentrate 2 and tailings 2; the concentrate 2 is subjected to the third concentration, and H 2 SO 4Adjust the pH of the slurry to 2.8-3.0 to obtain titanium concentrate and concentrate tailings; scavenge the roughing tailings, H 2 SO 4 The addition amount is 400±20g / t rougher tailings to obtain sweep concentrate and titanium tailings.
[0022] Among them, in the above-mentioned method for efficiently recovering ultrafine ilmenite in upgraded tailings, in step E, the TiO 2 The grade is 46.00-49.32%, and the recovery rate is 75%-85%.
[0023] In the present invention, the iron ore concentrate upgrading tailings are well-known minerals in the art, which are generally iron ore concentrate (grade 50-57%) obtained by beneficiation of vanadium-titanium magnetite, which are finely ground by a stirred mill (a horizontal stirred mill or a vertical stirred mill is also called a tower mill) and then enter weak magnetic separation to obtain upgraded iron ore concentrate and magnetic separation tailings, and the magnetic separation tailings are the iron ore concentrate upgrading tailings.
[0024] In the desulfurization roughing agent, titanium flotation roughing agent and titanium flotation selection agent of the present invention, H 2 SO 4 A sulfuric acid aqueous solution with a mass concentration of 10%-20% is used, and its dosage is calculated based on concentrated sulfuric acid.
[0025] The beneficial effects of the present invention are:
[0026] The present invention aims at the difficulties that the tailings from the upgraded iron ore contain ilmenite guest crystals, are of low grade and difficult to dissociate, and the like, optimizes the mineral processing technology, overcomes the problem that the degree of dissociation of monomers in the upgraded tailings gradually increases as the particle size becomes finer, improves the degree of dissociation of each particle size in the tailings from the upgraded iron ore, adjusts the reagent system, reduces titanium loss, and ultimately improves the grade and yield of the titanium concentrate, thereby realizing the recycling of the upgraded tailings that are currently difficult to utilize. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0028] Specifically, a method for recovering ultrafine titanium concentrate from tailings of vanadium-titanium magnetite concentrate includes the following steps:
[0029] A. Perform weak magnetic iron removal on the iron concentrate upgrading tailings with a magnetic field strength of 3000Gs to obtain iron concentrate and iron tailings;
[0030] B. The iron tailings obtained in step A are subjected to strong magnetic roughing. In the strong magnetic roughing, the diameter of the magnetic medium is 1.5 mm, the magnetic field strength is 1.2 T, the pulsation stroke is 2.5 CM, and the pulsation stroke is 300 times / min to obtain strong magnetic roughing concentrate and strong magnetic roughing tailings;
[0031] The strong magnetic roughing tailings are subjected to strong magnetic sweeping, in which the diameter of the concentrated magnetic medium is 2 mm, the magnetic field strength is 0.9 T, the pulsation stroke is 3 CM, and the pulsation frequency is 300 times / min, to obtain strong magnetic sweeping concentrate and strong magnetic sweeping tailings; the strong magnetic roughing concentrate and the strong magnetic sweeping concentrate are combined as strong magnetic concentrate;
[0032] C. Concentrating the strong magnetic concentrate obtained in step B by a cyclone to obtain cyclone sedimentation and cyclone overflow, and controlling the mass concentration of cyclone sedimentation to be 40% to 50%;
[0033] D. flotation desulfurization of the cyclone sediment obtained in step C to obtain desulfurized tailings and crude cobalt sulfide ore;
[0034] E. The desulfurization tailings obtained in step D are subjected to flotation separation to select titanium to obtain titanium concentrate and titanium-selected tailings.
[0035] In step A of the present invention, the TiO 2 The grade is 12-13.46%, and the -19μm content is 55-78%. The (4) type of fine-grained ilmenite in the iron ore upgrading tailings is a guest crystal of ilmenite finely ground from the iron ore. Its monomer dissociation degree is just opposite to that of the (1), (2), and (3) types of fine-grained ilmenite. As the particle size becomes finer, it gradually decreases. Therefore, its flotation grade is lower and the comprehensive recovery is more difficult. The present invention improves the dissociation degree of each particle size in the iron ore upgrading tailings by optimizing the mineral processing technology, thereby improving the grade and yield of the ilmenite concentrate.
[0036] In step B of the present invention, the TiO 2 The grade is 18.56~22.54%.
[0037] In step B of the present invention, the optimal concentration of the cyclone sand settling mass is controlled to be 40% to 50%. If the concentration is too low, it will lead to high dosage of reagents and low recovery rate; if it is too high, the loss in the desulfurization section will be large and the recovery rate will be reduced.
[0038] In step D of the present invention, the flotation desulfurization process is one roughing and two sweeping.
[0039] In the present invention, the cyclone sedimentation is directly used for subsequent flotation desulfurization and flotation titanium selection. At this time, the fine particle size of -800 mesh in the material is relatively high, so it is necessary to adjust the reagent system. According to the test, the present invention reduces the amount of xanthate and 2# oil in the desulfurization roughing stage to reduce the loss of titanium. Therefore, in step D of the present invention, in the flotation desulfurization, the amount of desulfurization roughing reagent used is: H 2 SO 4 800~1000g / t cyclone sand settling, 150~180g / t xanthate cyclone sand settling, 20~30g / t 2# oil cyclone sand settling.
[0040] In step E of the present invention, the process of titanium flotation separation is one roughing, three refining and one sweeping.
[0041] On the basis of the above desulfurization roughing, the present invention increases the dosage of reagents in the titanium flotation roughing stage according to the material characteristics. In step E, in the titanium flotation, the reagent system for titanium flotation roughing is: 2 SO 4 The dosage is 2000-2600g / t desulfurization tailings, the dosage of the adjusting agent is 200-400g / t desulfurization tailings, the dosage of the collecting agent is 2400-2800g / t desulfurization tailings, the dosage of the diesel is 500-700g / t desulfurization tailings, and the adjusting agent is composed of water glass, sodium tripolyphosphate and ethylenediaminetetraacetic acid (the proportion is the conventional proportion in this field).
[0042] In step E of the present invention, the specific operation of flotation titanium selection is: the desulfurization tailings obtained in step D are subjected to titanium flotation roughing to obtain a crude titanium concentrate and a roughing tailings; the crude titanium concentrate is subjected to a first concentration, and H is used before the first concentration. 2 SO 4 Adjust the pH of the slurry to 3.4-3.6 to obtain concentrate 1 and concentrate 1 tailings; conduct the second concentration of concentrate 1, and use H 2 SO 4 Adjust the pH of the slurry to 3.1-3.3 to obtain concentrate 2 and tailings 2; the concentrate 2 is subjected to the third concentration, and H 2 SO 4 Adjust the pH of the slurry to 2.8-3.0 to obtain titanium concentrate and concentrate tailings; scavenge the roughing tailings, H 2 SO 4 The addition amount is 400±20g / t rougher tailings to obtain sweep concentrate and titanium tailings.
[0043] In step E of the present invention, the TiO 2 The grade is 46.00-49.32%, and the recovery rate is 75%-85%.
[0044] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.
[0045] Example 1
[0046] The raw materials to be selected are the tailings of iron ore concentrate upgrading from a concentrator in Panzhihua, TiO 2 The grade is 13.73%, and the -19μm content is 78%. The specific implementation method is as follows:
[0047] 1. The raw materials are subjected to weak magnetic de-ironization with a magnetic field strength of 3000Gs to obtain iron concentrate and de-ironized tailings.
[0048] 2. The iron-removing tailings are subjected to a roughing and sweeping strong magnetic separation, wherein the diameter of the strong magnetic roughing medium is 1.5 mm, the magnetic field strength is 1.2 T, the pulsation stroke is 2.5 CM, and the pulsation frequency is 300 times / min. The diameter of the strong magnetic sweeping medium is 2 mm, the magnetic field strength is 0.9 T, the pulsation stroke is 3 CM, and the pulsation frequency is 300 times / min. The roughing concentrate and the sweeping concentrate are mixed as the strong magnetic concentrate. The strong magnetic concentrate TiO 2 The grade is 18.56% and the recovery rate is 81.34%.
[0049] 3. The strong magnetic concentrate is concentrated by a cyclone to obtain cyclone sand and cyclone overflow, and the cyclone sand concentration is controlled to be 42%.
[0050] 4. The above cyclone sand settling is subjected to one rough and two sweep desulfurization. The desulfurization is conventional existing technology. The dosage of desulfurization rough selection agent is: H 2 SO 4 800g / t, xanthate 180g / t, 2# oil 30g / t, to obtain crude cobalt sulfide ore and desulfurization tailings.
[0051] 5. The above desulfurized tailings are subjected to one roughing, three fines and one sweeping titanium selection, wherein the reagent system for the roughing titanium flotation selection is: H 2 SO 4 The dosage is 2000g / t, the dosage of the adjusting agent is 400g / t, the dosage of the collecting agent is 2400g / t, and the dosage of the diesel is 700g / t. The adjusting agent is composed of water glass, sodium tripolyphosphate and ethylenediaminetetraacetic acid. After the titanium flotation roughing, the crude titanium concentrate and the roughing tailings are obtained;
[0052] The crude titanium concentrate is first concentrated, and H 2 SO 4 Adjust the pH of the slurry to 3.5 to obtain concentrate 1 and concentrate 1 tailings. The concentrate 1 is subjected to a second concentration. H 2 SO 4 Adjust the pH of the slurry to 3.3 to obtain concentrate 2 and tailings 2. The concentrate 2 was subjected to the third concentration. 2 SO 4 Adjust the pH of the slurry to 3.0 to obtain the final titanium concentrate and concentrate 3 tailings, and the tailings are returned in sequence;
[0053] Rough tailings are scavenged and the reagent system is H 2 SO 4 400g / t, and obtain sweep concentrate and titanium tailings.
[0054] Finally, TiO 2 The flotation titanium concentrate has a grade of 47.32% and a recovery rate of 75.67%.
[0055] Table 1 Test results of raw material monomer dissociation degree
[0056] Granularity level / mesh Monomer dissociation degree / % 200-325 88.17 325-400 90.10 400-800 87.40 -800 85.98
[0057] As shown in Table 1, the monomer dissociation degree of the iron ore tailings raw material for upgrading the iron ore concentrate of the present invention decreases with decreasing particle size, which is contrary to the monomer dissociation degree-particle size law of the traditional material. This shows that the raw material of the present invention is the guest crystal mineral ground out of the vanadium-titanium magnetite concentrate after fine grinding, which is completely different from the properties of the fine particles appearing in the existing traditional process. The mineral processing process of the present invention can significantly improve the dissociation degree of each particle size, thereby providing TiO 2 Grade and recovery.
Claims
1. A method for recovering ultrafine titanium concentrate from tailings of vanadium-titanium magnetite concentrate, characterized in that: The following steps are involved: A. Perform weak magnetic iron removal on the iron concentrate upgrading tailings with a magnetic field strength of 3000Gs to obtain iron concentrate and iron tailings; B. The iron tailings obtained in step A are subjected to strong magnetic roughing. In the strong magnetic roughing, the diameter of the magnetic medium is 1.5 mm, the magnetic field strength is 1.2 T, the pulsation stroke is 2.5 CM, and the pulsation stroke is 300 times / min to obtain strong magnetic roughing concentrate and strong magnetic roughing tailings; The strong magnetic roughing tailings are subjected to strong magnetic sweeping, in which the diameter of the concentrated magnetic medium is 2 mm, the magnetic field strength is 0.9 T, the pulsation stroke is 3 CM, and the pulsation frequency is 300 times / min, to obtain strong magnetic sweeping concentrate and strong magnetic sweeping tailings; the strong magnetic roughing concentrate and the strong magnetic sweeping concentrate are combined as strong magnetic concentrate; C. Concentrating the strong magnetic concentrate obtained in step B by a cyclone to obtain cyclone sedimentation and cyclone overflow, and controlling the mass concentration of cyclone sedimentation to be 40% to 50%; D. flotation desulfurization of the cyclone sediment obtained in step C to obtain desulfurized tailings and coarse sulfur-cobalt ore; E. The desulfurization tailings obtained in step D are subjected to flotation separation for titanium separation to obtain titanium concentrate and titanium separation tailings.
2. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 1, characterized in that: In step A, the TiO2 grade of the iron ore upgrading tailings is 12-13.46%, and the -19 μm content is 55-78%.
3. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 1, characterized in that: In step B, the TiO2 grade of the obtained strong magnetic concentrate is 18.56-22.54%.
4. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 1, characterized in that: In step D, the flotation desulfurization process is one roughing and two sweeping.
5. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 4, characterized in that: In step D, in flotation desulfurization, the dosage of desulfurization roughing reagents is: H2SO4 800-1000g / t cyclone sand settling, xanthate 150-180g / t cyclone sand settling, 2# oil 20-30g / t cyclone sand settling.
6. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 1, characterized in that: In step E, the process of titanium flotation separation is one roughing, three fines and one sweeping.
7. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 6, characterized in that: In step E, in the flotation separation of titanium, the reagent system for the rough selection of flotation titanium is: H2SO4 dosage 2000-2600g / t desulfurization tailings, adjusting agent dosage 200-400g / t desulfurization tailings, collector dosage 2400-2800g / t desulfurization tailings, diesel dosage 500-700g / t desulfurization tailings, and the adjusting agent is composed of water glass, sodium tripolyphosphate and ethylenediaminetetraacetic acid.
8. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to claim 6 or 7, characterized in that: In step E, the specific operation of flotation titanium selection is as follows: the desulfurization tailings obtained in step D are subjected to titanium flotation roughing to obtain a crude titanium concentrate and a roughing tailing; the crude titanium concentrate is subjected to a first concentration, and the pH of the slurry is adjusted to 3.4-3.6 by H2SO4 before the first concentration to obtain a concentrate 1 and a concentrate 1 tailing; the concentrate 1 concentrate is subjected to a second concentration, and the pH of the slurry is adjusted to 3.1-3.3 by H2SO4 before the second concentration to obtain a concentrate 2 and a concentrate 2 tailing; the concentrate 2 concentrate is subjected to a third concentration, and the pH of the slurry is adjusted to 2.8-3.0 by H2SO4 before the third concentration to obtain a titanium concentrate and a concentrate 3 tailing; the roughing tailings are subjected to scavenging, and the amount of H2SO4 added is 400±20g / t of the roughing tailings to obtain a scavenging concentrate and a titanium tailing.
9. The method for efficiently recovering ultrafine ilmenite in upgraded tailings according to any one of claims 1 to 8, characterized in that: In step E, the TiO2 grade of the obtained titanium concentrate is 46.00-49.32%, and the recovery rate is 75%-85%.
Citation Information
Patent Citations
Recycling method of ultra-micro-fine-particle ilmenite
CN112871437A
System and method for beneficiation of ultra-fine particle ilmenite
CN115301400A
Cited By
Process for recovering ultra-fine particle ilmenite
CN121372665A