Surface treatment method for heat-insulating and corrosion-resistant aluminum alloy doors and windows

Through the combination of resin primer, solar heat-absorbing coating and fast-drying water-based coatings, combined with ultraviolet irradiation and drying technology, the problem that aluminum alloy doors and windows easily fall off at high temperatures and difficult to quickly heat up at low temperatures is achieved, achieving better Thermal insulation and durability.

CN119076347APending Publication Date: 2024-12-06ANHUI GAODE ALUMINUM
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410957170.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-06

Smart Images

  • Figure CN119076347A_ABST
    Figure CN119076347A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy door and window surface treatment, and discloses a heat-insulation and corrosion-resistant aluminum alloy door and window surface treatment method which comprises the following steps: step 1, grinding and polishing a formed aluminum alloy door and window frame, removing surface welding impurities, and then cleaning and drying; secondly, the aluminum alloy doors and windows are subjected to acid pickling, and after acid pickling is completed, the aluminum alloy doors and windows are cleaned and subjected to anodic oxidation operation; thirdly, resin primer is sprayed to the aluminum alloy door and window obtained after anodic oxidation is completed, and natural drying is conducted after spraying is completed; fourthly, the solar heat absorption coating is used for spraying the aluminum alloy door and window, and secondary spraying is conducted after primary spraying and drying are completed; fifthly, the surfaces of the aluminum alloy doors and windows dried in the fourth step are coated with quick-drying water-based paint to serve as protective layers; and 6, the aluminum alloy door and window coated with the quick-drying water-based paint is irradiated through ultraviolet rays to be dried, and a finished product is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface treatment of aluminum alloy doors and windows, and in particular to a surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows. Background Art

[0002] Aluminum alloy doors and windows refer to doors and windows made of aluminum alloy extruded profiles as frames, stiles, and sashes. Aluminum alloy windows are beautiful, sealed, and high in strength. They are widely used in the field of construction engineering. The surface of aluminum alloy is oxidized to be smooth and shiny. The window frame is large and can be inlaid with a large area of ​​glass, allowing sufficient and bright light in the room, enhancing the virtual and real contrast between the indoor and outdoor facades, and making the room more layered; aluminum alloy itself is easy to extrude, the cross-sectional dimensions of the profile are precise, and the processing accuracy is high. Therefore, many owners choose to use aluminum alloy doors and windows in decoration.

[0003] After searching, it was found that the prior art publication number is CN 108166904 A, which is a heat-insulating and corrosion-resistant aluminum alloy door and window surface treatment method, which includes nine steps in total. The present invention uses the method of assembling and polishing first and then coating to treat the outer surface of the aluminum alloy door and window, avoiding damage to the outer surface coating layer during the assembly process and ensuring the integrity of the coating layer; the layer-by-layer coating method ensures that each functional layer will not penetrate each other, ensuring the functionality of the coating layer; using laser for annealing treatment, the operation is more flexible and no large annealing equipment is required; the heat insulation layer is set in the middle to effectively prevent the annealing heat from being transferred to the aluminum alloy door and window, effectively protecting the aluminum alloy door and window.

[0004] Although the above-mentioned technical solution uses laser for annealing treatment, the raw materials used in the layer-by-layer coating method are still traditional coatings. Aluminum is one of the materials with extremely fast thermal conductivity. Aluminum alloy doors and windows are installed on the exterior walls. In summer, direct sunlight seriously affects the activity of the coating, causing the coating to fall off. At the same time, due to the material limitations of the coating and the glass screen, the temperature of aluminum alloy doors and windows is difficult to rise quickly in winter, which makes it difficult for users to open and close the doors and windows. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a method for surface treatment of heat-insulating and corrosion-resistant aluminum alloy doors and windows, which has the advantages that the coating of aluminum alloy doors and windows is not easy to fall off during the high temperature period in summer, and the aluminum alloy doors and windows can quickly absorb heat and increase the temperature during the low temperature in winter, thereby solving the problems of the above-mentioned technologies.

[0007] (II) Technical solution

[0008] To achieve the above object, the present invention provides the following technical solution: a surface treatment method for heat-insulating and corrosion-resistant aluminum alloy doors and windows, comprising the following steps:

[0009] Step 1: Grind and polish the formed aluminum alloy door and window frames, remove surface welding impurities, clean and dry them;

[0010] Step 2: pickling the aluminum alloy doors and windows, washing them after pickling and performing anodizing operation;

[0011] Step 3: Spray resin primer on the anodized aluminum alloy doors and windows, and let it dry naturally after spraying;

[0012] Step 4: Use solar heat-absorbing paint to spray aluminum alloy doors and windows, and spray a second time after the first spray is dried;

[0013] Step 5: coating the surface of the aluminum alloy doors and windows dried in step 4 with a quick-drying water-based paint as a protective layer;

[0014] Step 6: Use ultraviolet rays to irradiate the aluminum alloy doors and windows coated with quick-drying water-based paint to dry them and obtain the finished product.

[0015] Preferably, the grinding and polishing of aluminum alloy doors and windows in step 1 further includes the following detailed steps:

[0016] S1.1. Place the aluminum alloy door and window frame on the automatic grinding machine and set the parameters for grinding and polishing;

[0017] S1.2. After grinding and polishing, the aluminum alloy door and window frames are transported to the workstation for removing welding impurities to remove impurities at the welding points;

[0018] S1.3. Move the treated aluminum alloy door and window frames to the cleaning equipment for surface cleaning;

[0019] S1.4. After cleaning, move the aluminum alloy door and window frames to a dry area and dry them using a fan or drying equipment;

[0020] S1.5. Check whether the surface is smooth and free of defects, and whether the welding point is flat.

[0021] Preferably, the parameters in S1.1 include grinding speed, grinding pressure and grinding wheel particle size, the grinding speed is 300 / rpm-1000 / rpm, the grinding pressure is 1 MPa-3 MPa, and the grinding wheel particle size is 200 mesh-400 mesh.

[0022] Preferably, the step 2 further includes the following detailed steps:

[0023] S2.1. Place the aluminum alloy doors and windows in the pickling tank in batches until they are completely soaked;

[0024] S2.2, adjust the pickling concentration to 3%-16%, the pickling temperature to 20℃-60℃ and the pickling time to 5min-20min;

[0025] S2.3. After the pickling is completed, the aluminum alloy doors and windows are moved to the neutralization tank, and the residual pickling agent is neutralized with a neutralizer. Then the doors and windows are moved to the cleaning tank and the surface is cleaned with a cleaning agent.

[0026] S2.4. Move the treated aluminum alloy doors and windows into the anodizing tank, ensure complete immersion, and start the equipment for anodizing;

[0027] S2.5. After anodizing is completed, move the doors and windows to the neutralization tank for acid neutralization, and then move them to the cleaning tank for thorough cleaning.

[0028] Preferably, the concentration of the anodizing agent in S2.4 is 5%-20%, and the current density is 1A / dm 2 -3A / dm 2 The treatment time is 5min-16min, and the anodizing agent in S2.4 is sulfuric acid electrolyte, chromium sulfate electrolyte, magnesium sulfate electrolyte and citric acid electrolyte.

[0029] Preferably, the solar heat-absorbing coating in step 4 is a resin primer, and the resin primer further comprises the following detailed steps:

[0030] S3.1. Place the aluminum alloy doors and windows on the brackets or hangers in the spraying area to ensure that the surfaces of the doors and windows are clean and dust-free;

[0031] S3.2. Use spraying equipment to evenly spray the resin primer on the surface of aluminum alloy doors and windows to ensure that the primer covers evenly without any missing parts;

[0032] S3.3. After spraying, place the aluminum alloy doors and windows in a well-ventilated area for natural drying. The natural drying time of the resin primer is 5h-26h;

[0033] S3.4. Check whether the coating surface is flat, and whether there is any missing coating, peeling or blistering. If the above problems are found, repair or re-spray.

[0034] Preferably, the resin primer in step 4 includes alkyd resin primer, epoxy resin primer, polyurethane primer, acrylic resin primer and modified silicone primer.

[0035] Preferably, the step of applying the five quick-drying water-based paints further comprises the following steps:

[0036] S4.1. Load the dried aluminum alloy doors and windows onto the conveyor belt or rack of the production line;

[0037] S4.2. Prepare the paint and load it into the spraying equipment. The automatic spraying system will evenly coat the quick-drying water-based paint on the surface of the aluminum alloy doors and windows;

[0038] S4.3, the coating thickness is 0.1mm-0.2mm. After coating, the doors and windows enter the drying area through the conveyor belt;

[0039] S4.4. In the drying area, hot air or infrared rays are used to accelerate the drying of the paint.

[0040] Preferably, the quick-drying water-based paint is prepared by mixing one or more of acrylic water-based paint, epoxy water-based paint, polyurethane water-based paint, water-based baking varnish and water-based anti-rust paint.

[0041] Preferably, the ultraviolet drying power in step 6 is 100-300 watts / cm 2 , the drying time is 1min-3min.

[0042] Compared with the prior art, the present invention provides a heat-insulating and corrosion-resistant aluminum alloy door and window surface treatment method, which has the following beneficial effects:

[0043] 1. The present invention provides an additional protective layer through resin primer and solar heat-absorbing coating, thereby enhancing the thermal insulation and durability of doors and windows. These coatings can resist high temperature and ultraviolet radiation, reduce heat absorption on the surface of doors and windows, and thus reduce coating shedding. Quick-drying water-based coatings have the characteristics of rapid curing and can form a strong coating in a short time. This coating usually has high adhesion and durability, can effectively protect the surface of doors and windows from environmental influences, and accelerates the curing process of the coating by drying under ultraviolet radiation, ensuring that the coating can be quickly formed and has sufficient hardness and durability. This rapid curing process helps to improve the production efficiency of doors and windows, and ensures that the coating is not easy to fall off in a high temperature environment, achieving the beneficial effect that the coating of aluminum alloy doors and windows is not easy to fall off during the high temperature period in summer.

[0044] 2. The present invention uses solar heat-absorbing paint to spray aluminum alloy doors and windows. This paint usually has a high heat absorption performance, can quickly absorb heat in the sun, and convert it into heat energy for doors and windows. At the same time, in step six, the resin primer coated by ultraviolet irradiation also has heat absorption characteristics, further increasing the heat absorption effect of doors and windows, achieving the beneficial effect of aluminum alloy doors and windows being able to quickly absorb heat and increase temperature at low temperatures in winter. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a schematic diagram of the structure of the present invention; DETAILED DESCRIPTION

[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] See also Figure 1 A method for treating the surface of heat-insulating and corrosion-resistant aluminum alloy doors and windows comprises the following steps:

[0048] Step 1: Grind and polish the formed aluminum alloy door and window frames, remove surface welding impurities, clean and dry them;

[0049] Step 2: pickling the aluminum alloy doors and windows, washing them after pickling and performing anodizing operation;

[0050] Step 3: Spray resin primer on the anodized aluminum alloy doors and windows, and let it dry naturally after spraying;

[0051] Step 4: Use solar heat-absorbing paint to spray aluminum alloy doors and windows, and spray a second time after the first spray is dried;

[0052] Step 5: coating the surface of the aluminum alloy doors and windows dried in step 4 with a quick-drying water-based paint as a protective layer;

[0053] Step 6: Use ultraviolet rays to irradiate the aluminum alloy doors and windows coated with quick-drying water-based paint to dry them and obtain the finished product.

[0054] By using resin primer and quick-drying water-based paint as the coating, and drying it with ultraviolet light, it can be ensured that the coating is firm, uniform, and not easy to fall off. The use of water-based paint and ultraviolet drying technology reduces the emission of volatile organic compounds (VOCs), meets environmental protection requirements, and also improves the safety of the construction process. The use of quick-drying water-based paint and ultraviolet drying technology accelerates the curing process of the coating.

[0055] Preferably, the grinding and polishing of aluminum alloy doors and windows in step 1 further includes the following detailed steps:

[0056] S1.1. Place the aluminum alloy door and window frame on the automatic grinding machine and set the parameters for grinding and polishing;

[0057] S1.2. After grinding and polishing, the aluminum alloy door and window frames are transported to the workstation for removing welding impurities to remove impurities at the welding points;

[0058] S1.3. Move the treated aluminum alloy door and window frames to the cleaning equipment for surface cleaning;

[0059] S1.4. After cleaning, move the aluminum alloy door and window frames to a dry area and dry them using a fan or drying equipment;

[0060] S1.5. Check whether the surface is smooth and free of defects, and whether the welding point is flat.

[0061] By placing it on an automated grinder for grinding and polishing, the production process is automated, production efficiency and consistency are improved, and labor costs are reduced. Impurities are removed and cleaned at the workstation for removing welding impurities, which can fully clean the surface of the door and window frames and ensure adhesion and surface quality after coating.

[0062] Preferably, the parameters in S1.1 include grinding speed, grinding pressure and grinding wheel particle size, the grinding speed is 300 / rpm-1000 / rpm, the grinding pressure is 1 MPa-3 MPa, and the grinding wheel particle size is 200 mesh-400 mesh.

[0063] It is suitable for the initial removal of large particles and rough parts on the surface of doors and windows to avoid unnecessary surface damage caused by too fast a speed.

[0064] Preferably, the step 2 further includes the following detailed steps:

[0065] S2.1. Place the aluminum alloy doors and windows in the pickling tank in batches until they are completely soaked;

[0066] S2.2, adjust the pickling concentration to 3%-16%, the pickling temperature to 20℃-60℃ and the pickling time to 5min-20min;

[0067] S2.3. After the pickling is completed, the aluminum alloy doors and windows are moved to the neutralization tank, and the residual pickling agent is neutralized with a neutralizer. Then the doors and windows are moved to the cleaning tank and the surface is cleaned with a cleaning agent.

[0068] S2.4. Move the treated aluminum alloy doors and windows into the anodizing tank, ensure complete immersion, and start the equipment for anodizing;

[0069] S2.5. After anodizing is completed, move the doors and windows to the neutralization tank for acid neutralization, and then move them to the cleaning tank for thorough cleaning.

[0070] Preferably, the concentration of the anodizing agent in S2.4 is 5%-20%, and the current density is 1A / dm 2 -3A / dm 2 The treatment time is 5min-16min, and the anodizing agent in S2.4 is sulfuric acid electrolyte, chromium sulfate electrolyte, magnesium sulfate electrolyte and citric acid electrolyte.

[0071] Preferably, the solar heat-absorbing coating in step 4 is a resin primer, and the resin primer further comprises the following detailed steps:

[0072] S3.1. Place the aluminum alloy doors and windows on the brackets or hangers in the spraying area to ensure that the surfaces of the doors and windows are clean and dust-free;

[0073] S3.2. Use spraying equipment to evenly spray the resin primer on the surface of aluminum alloy doors and windows to ensure that the primer covers evenly without any missing parts;

[0074] S3.3. After spraying, place the aluminum alloy doors and windows in a well-ventilated area for natural drying. The natural drying time of the resin primer is 5h-26h;

[0075] S3.4. Check whether the coating surface is flat, and whether there is any missing coating, peeling or blistering. If the above problems are found, repair or re-spray.

[0076] Resin primer can firmly adhere to the aluminum alloy surface to form a solid base layer, providing a good foundation for subsequent coatings and enhancing the adhesion and stability of the coatings. Resin primer can effectively prevent the surface of aluminum alloy doors and windows from corrosion and oxidation, extend the service life of doors and windows, and reduce maintenance costs.

[0077] Preferably, the resin primer in step 4 includes alkyd resin primer, epoxy resin primer, polyurethane primer, acrylic resin primer and modified silicone primer.

[0078] Preferably, the step of applying the five quick-drying water-based paints further comprises the following steps:

[0079] S4.1. Load the dried aluminum alloy doors and windows onto the conveyor belt or rack of the production line;

[0080] S4.2. Prepare the paint and load it into the spraying equipment. The automatic spraying system will evenly coat the quick-drying water-based paint on the surface of the aluminum alloy doors and windows;

[0081] S4.3, the coating thickness is 0.1mm-0.2mm. After coating, the doors and windows enter the drying area through the conveyor belt;

[0082] S4.4. In the drying area, hot air or infrared rays are used to accelerate the drying of the paint.

[0083] Preferably, the quick-drying water-based paint is prepared by mixing one or more of acrylic water-based paint, epoxy water-based paint, polyurethane water-based paint, water-based baking varnish and water-based anti-rust paint.

[0084] Preferably, the ultraviolet drying power in step 6 is 100-300 watts / cm 2 , the drying time is 1min-3min.

[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and alterations may be made to the embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for treating the surface of heat-insulating and corrosion-resistant aluminum alloy doors and windows, characterized in that: The following steps are involved: Step 1: Grind and polish the formed aluminum alloy door and window frames, remove surface welding impurities, clean and dry them; Step 2: pickling the aluminum alloy doors and windows, washing them after pickling and performing anodizing operation; Step 3: Spray resin primer on the anodized aluminum alloy doors and windows, and let it dry naturally after spraying; Step 4: Use solar heat-absorbing paint to spray aluminum alloy doors and windows, and spray a second time after the first spray is dried; Step 5: coating the surface of the aluminum alloy doors and windows dried in step 4 with a quick-drying water-based paint as a protective layer; Step 6: Use ultraviolet rays to irradiate the aluminum alloy doors and windows coated with quick-drying water-based paint to dry them and obtain the finished product.

2. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized in that: The step 1 of grinding and polishing the aluminum alloy doors and windows also includes the following detailed steps: S1.

1. Place the aluminum alloy door and window frame on the automatic grinding machine and set the parameters for grinding and polishing; S1.

2. After grinding and polishing, the aluminum alloy door and window frames are transported to the workstation for removing welding impurities to remove impurities at the welding points; S1.

3. Move the treated aluminum alloy door and window frames to the cleaning equipment for surface cleaning; S1.

4. After cleaning, move the aluminum alloy door and window frames to a dry area and dry them using a fan or drying equipment; S1.

5. Check whether the surface is smooth and free of defects, and whether the welding point is flat.

3. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 2 is characterized in that: The parameters in S1.1 include grinding speed, grinding pressure and grinding wheel particle size. The grinding speed is 300 / rpm-1000 / rpm, the grinding pressure is 1 MPa-3 MPa, and the grinding wheel particle size is 200 mesh-400 mesh.

4. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized in that: The step 2 also includes the following detailed steps: S2.

1. Place the aluminum alloy doors and windows in the pickling tank in batches until they are completely soaked; S2.2, adjust the pickling concentration to 3%-16%, the pickling temperature to 20℃-60℃ and the pickling time to 5min-20min; S2.

3. After the pickling is completed, the aluminum alloy doors and windows are moved to the neutralization tank, and the residual pickling agent is neutralized with a neutralizer. Then the doors and windows are moved to the cleaning tank and the surface is cleaned with a cleaning agent. S2.

4. Move the treated aluminum alloy doors and windows into the anodizing tank, ensure complete immersion, and start the equipment for anodizing; S2.

5. After anodizing is completed, move the doors and windows to the neutralization tank for acid neutralization, and then move them to the cleaning tank for thorough cleaning.

5. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 4 is characterized in that: The concentration of the anodizing agent in S2.4 is 5%-20%, and the current density is 1A / dm 2 -3A / dm 2 The treatment time is 5min-16min, and the anodizing agent in S2.4 is sulfuric acid electrolyte, chromium sulfate electrolyte, magnesium sulfate electrolyte and citric acid electrolyte.

6. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized in that: The solar heat-absorbing coating in step 4 is a resin primer, and the resin primer also includes the following detailed steps: S3.

1. Place the aluminum alloy doors and windows on the brackets or hangers in the spraying area to ensure that the surfaces of the doors and windows are clean and dust-free; S3.

2. Use spraying equipment to evenly spray the resin primer on the surface of aluminum alloy doors and windows to ensure that the primer covers evenly without any missing parts; S3.

3. After spraying, place the aluminum alloy doors and windows in a well-ventilated area for natural drying. The natural drying time of the resin primer is 5h-26h; S3.

4. Check whether the coating surface is flat, and whether there is any missing coating, peeling or blistering. If the above problems are found, repair or re-spray.

7. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized by: The resin primer in step 4 includes alkyd resin primer, epoxy resin primer, polyurethane primer, acrylic resin primer and modified silicone primer.

8. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized by: The five steps of applying the quick-drying water-based paint also include the following steps: S4.

1. Load the dried aluminum alloy doors and windows onto the conveyor belt or rack of the production line; S4.

2. Prepare the paint and load it into the spraying equipment. The automatic spraying system will evenly coat the quick-drying water-based paint on the surface of the aluminum alloy doors and windows; S4.3, the coating thickness is 0.1mm-0.2mm. After coating, the doors and windows enter the drying area through the conveyor belt; S4.

4. In the drying area, hot air or infrared rays are used to accelerate the drying of the paint.

9. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized by: The quick-drying water-based paint is prepared by mixing one or more of acrylic water-based paint, epoxy water-based paint, polyurethane water-based paint, water-based baking varnish and water-based anti-rust paint.

10. The surface treatment method of heat-insulating and corrosion-resistant aluminum alloy doors and windows according to claim 1 is characterized in that: The ultraviolet drying power in step 6 is 100-300 watts / cm 2 , the drying time is 1min-3min.

Citation Information

Patent Citations

  • Coating process method for waterborne coating

    CN107377335A

  • Anti-corrosion coating for hydraulic engineering gate protective coating layer and spraying method thereof

    CN107384121A

  • Treatment method for surface of heat-insulation corrosion-resistant aluminum alloy door and window

    CN112138962A

  • Aluminum profile spraying process

    CN117339847A

  • Aluminum alloy door and window with good wear-resistant effect

    CN213807264U