Online sorbite production process for hot-rolled high-speed wire rod
Through the online Sortenitization production process of hot-rolled high-speed wires, the conversion of austenite to sonitite by using rapid cooling and air-cooled roller insulation, the problems of low Sortenitization rate and high production cost in traditional processes are solved, and the problem of low Sortenitization rate and high production cost in traditional processes is achieved. High-strength and high-performance hot-rolled strip production.
Patent Information
- Application Number
- CN202411338485.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-25
AI Technical Summary
In traditional high-line and large-disk coil rolling processes, the sonitization rate is high, but the production cost is high, the energy consumption is increased, and the product quality is poor, making it difficult to control the through-bar temperature and performance.
Using hot-rolled high-speed wire online skeinitization production process, including rolling, rapid cooling, low-temperature wire spinning, online skeinitization and PF line cooling, it is cooled through multi-section annular venturi nozzles, and the surface temperature of the rolled piece is controlled at 550. -650℃, so that the soxunite content is ≥92%, and the austenite to soxunite is transformed in thermal insulation on the air-cooled roller.
It realizes high-strength and high-performance hot-rolled strips, reduces production costs, improves product stability and purity, and meets the requirements of high-strength steel cords and building steel.
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-speed wire and large coil rolling, and in particular to an on-line sintering production process and device for hot-rolled high-speed wire. Background Art
[0002] With the development of lightweight materials and the continuous improvement of environmental protection requirements for industrial wire materials, they are gradually developing towards high strength and high performance. In particular, the processing procedures of cord steel are complicated, and the total reduction rate of wire rods after multiple drawing processes exceeds 99.0%, which is close to the limit of the drawing process, so the requirements for the troostitization rate of wire rods are extremely high.
[0003] Traditional production processes often require hot rolling online salt bath or offline salt bath troostitization treatment, which increases energy consumption and production costs. Or a large air volume cooling process is used on the Stelmor air cooling line, but the product quality stability is not high, especially the temperature and performance of the rod are often poor and the control indicators cannot be achieved.
[0004] Therefore, it has become an urgent requirement to further optimize and adjust the production and processing procedures of hot-rolled high-speed wire and large coil in-line calcination, to achieve the control of material structure under the optimal supercooling and temperature combination conditions, to improve production stability, reduce costs and improve product competitiveness. Summary of the invention
[0005] In order to overcome the above-mentioned defects, the object of the present invention is to provide an on-line sorbite production process for hot-rolled high-speed wire rod, so as to effectively and stably increase the sorbite structure content and control the stability.
[0006] To achieve the above-mentioned object, the present invention provides an on-line sintering production process for hot-rolled high-speed wire rods, the process comprising: rolling, rapid cooling, low-temperature wire drawing, on-line sintering, coiling and PF line cooling:
[0007] The rapid cooling step: the cooling capacity of the water tank is set to be not less than 350°C, the surface temperature of the rolled piece is controlled to be not less than 550°C, the wire drawing or coiling temperature is 600-650°C, and the temperature difference of the same batch of rolling is ±15°C.
[0008] Furthermore, the rapid cooling refers to reducing the temperature of the rolled piece to the sorbite production temperature range of 600-650° C. within 3 seconds.
[0009] Furthermore, the steps of on-line suturing are specifically as follows:
[0010] The high-speed wire is kept warm on the air-cooling line for 30-150s after passing through the spinning machine or being coiled. The front 25-45m of the insulation cover is completely closed and the roller running speed is 0.2-2m / s. The insulation duration on the air-cooling roller is 30-150s to complete the transformation of the wire product from austenite to sorbite, and the sorbite content is ≥92%.
[0011] Furthermore, the coiling and PF line cooling are completed in air to below 80°C, which is convenient for inspection and sampling, cutting and storage.
[0012] Furthermore, the wire coil is cooled on the PF line for no less than 20 minutes after being wound.
[0013] Furthermore, the rolling process is as follows: adopting two processes, austenite zone rolling and dual-phase zone rolling, the final rolling deformation is controlled at 30-60%; the final rolling pass has a rolling temperature of Ar1-Ar3 or Ar1-Arcm in the dual-phase zone, and the rolling temperature difference of the same batch is ±15°C; the final rolling pass has a rolling temperature of Ar3-1000°C in the austenite zone, and the rolling temperature difference of the same batch is ±15°C.
[0014] Furthermore, the rapid cooling process adopts a multi-stage annular venturi nozzle, 6-9 groups of which are placed in a closed box, and the outlet and inlet are water-sealed and air-sealed to prevent steam and water from being brought out of the water tank; 3-5 sets of such water tanks are provided, and the cooling capacity is not less than 350°C; a surface detection device is provided in the cooling zone to control the surface temperature of the rolled piece to be not lower than 550°C, the wire drawing or coiling temperature is 600-650°C, and the temperature difference of the same batch of rolling is ±15°C.
[0015] The present invention controls the generation of internal sorbite structure by controlling the processes of heating, rolling, rapid cooling, on-line sorbite treatment and PF line cooling in the high-speed wire production process, thereby improving the strength, plasticity, toughness and drawing properties of the material. The sorbite rate of the hot-rolled wire rod produced by the present invention is ≥92%, there is no large-scale network cementite and proeutectoid ferrite, and it has a high purity, which can meet the requirements of ultra-high strength steel cord drawing and low alloy composition of construction steel. DETAILED DESCRIPTION
[0016] In the description of the present invention, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships as shown, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0017] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0018] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0019] The purpose of the rolling process of the present invention is to obtain a fine-grained and uniform rolled structure by rolling the steel in the low-temperature austenite zone or the two-phase zone in the final rolling pass. The rolling deformation temperature is reduced, the stability of the supercooled austenite is reduced, and the structure is prepared for the formation of sorbite. Therefore, the final rolling deformation is controlled at 30-60%; the rolling temperature in the two-phase zone is Ar1-Ar3 or Ar1-Arcm, and the rolling temperature difference of the same batch is ±15°C; the rolling temperature in the austenite zone is Ar3-1000°C, and the rolling temperature difference of the same batch is ±15°C.
[0020] The sorbite treatment is designed to be three stages: the first stage is rapid cooling, the cooling capacity of the water tank is set to be no less than 350℃, the surface temperature of the rolled piece is controlled to be no less than 550℃, the wire drawing or coiling temperature is 600-650℃, and the temperature difference of the same batch of rolling is ±15℃. The temperature of the rolled piece is quickly reduced to the sorbite production temperature range of 600-650℃ within 3s. And by controlling the surface temperature, other tissue states are prevented from being generated.
[0021] The second stage is to complete the sorbite transformation in the range of 600-650℃. After the high-speed wire passes through the spinning machine or coiling, it is kept warm on the air cooling line for 30-150s, the front section of the insulation cover is completely closed for 25-45m, and the roller running speed is 0.2-2m / s. The insulation duration on the air cooling roller is 30-150s, so that the wire product completes the transformation from austenite structure to sorbite, and the sorbite content is ≥92%.
[0022] The third stage is coil collection and PF line cooling, which is completed in the air cooling to below 80℃, which is convenient for inspection sampling, cutting and storage. After the coil is collected, it continues to cool in the PF line, and the cooling time is not less than 20 minutes.
[0023] In the above-mentioned hot-rolled high-speed wire rod production process of wire calcination, the product has a hot-rolled high-speed wire or large coil with a diameter of Φ4.0-45mm.
[0024] Specifically, the in-line troostitizing production process of hot-rolled high-speed wire rod of the present invention comprises the steps of heating, rolling, rapid cooling, low-temperature wire laying, in-line troostitizing, coiling and PF line cooling; wherein, the final rolling temperature is 750-1000°C; followed by multiple rapid cooling, and the surface temperature is controlled to be not less than 550°C; the wire laying temperature is 600-650°C, and the insulation duration on the air-cooled roller is 30-150s, so that the wire rod product completes the transformation from austenite structure to troostite, and the troostite content is ≥92%.
[0025] The rolling process adopts two processes, austenite zone rolling and dual-phase zone rolling, and the final rolling deformation is controlled at 30-60%; the rolling temperature of the final rolling pass in the dual-phase zone is Ar1-Ar3 or Ar1-Arcm, and the rolling temperature difference of the same batch is ±15°C; the rolling temperature of the final rolling pass in the austenite zone is Ar3-1000°C, and the rolling temperature difference of the same batch is ±15°C.
[0026] The rapid cooling process adopts a multi-section annular venturi nozzle, 6-9 groups of which are placed in a closed box, and the outlet and inlet are water-sealed and air-sealed to prevent steam and water from being carried out of the water tank; 3-5 sets of such water tanks are provided, and the cooling capacity is not less than 350°C; a surface detection device is provided in the cooling zone to control the surface temperature of the rolled piece to be not less than 550°C, the wire drawing or coiling temperature is 600-650°C, and the temperature difference of the same batch of rolling is ±15°C.
[0027] The on-line wire calcining process is characterized in that the high-speed wire is kept warm on the air cooling line for 30-150s after being coiled by the spinning machine, the front section 25-45m of the insulation cover is completely closed, and the roller running speed is 0.2-2m / s.
[0028] The wire coils are further cooled on the PF line after being wound up, and the cooling time is not less than 20 minutes.
[0029] Example 1
[0030] The in-line wire sintering production process for hot-rolled high-speed wire of this embodiment includes the following steps.
[0031] (1) Rolling: The entire rolling process adopts continuous twist-free rolling, with 4 final rolling passes, including 2 reducing mills and 2 sizing mills; the section size before rolling is Φ12.5mm, the size of the rolled product is Φ10.0mm, and the final rolling temperature is 850-880℃.
[0032] (2) In-line wire calcining treatment: After rolling, open three water tanks to control the surface temperature of the rolled piece to be no less than 550°C, and send it to the spinning machine within 3 seconds, with a spinning temperature of 630-650°C; after the high-speed wire is coiled by the spinning machine, keep it warm on the air cooling line for 60 seconds, and the front 40m of the insulation cover is completely closed, and the operation of the first to ninth rollers is gradually increased, with a speed of 0.2-0.8m / s.
[0033] (3) The diameter of the bar in this embodiment is Φ10.0 mm, and the chemical composition is C: 0.85-0.90%, Mn: 0.40-0.60%, Si: 0.15-0.30%, P: ≤0.012%, S: ≤0.012%, O≤0.0020%, [N]≤0.0045%, and the balance is Fe and unavoidable impurities. The hot-rolled structure is mainly troostite, with a content of ≥92% and a grain size of 9.0.
[0034] Example 2
[0035] The in-line wire sintering production process for hot-rolled high-speed wire of this embodiment includes the following steps.
[0036] (1) Rolling: The entire rolling process adopts continuous twist-free rolling, with 4 final rolling passes, including 2 reducing mills and 2 sizing mills; the section size before rolling is Φ11.5mm, the size of the rolled product is Φ8.0mm, and the final rolling temperature is 750-780℃.
[0037] (2) In-line wire calcining treatment: After rolling, two water tanks are opened to control the surface temperature of the rolled piece to be no less than 550°C. The rolled piece is sent to the spinning machine within 3 seconds, and the spinning temperature is 600-630°C. After the high-speed wire is coiled by the spinning machine, it is kept warm on the air cooling line for 30 seconds. The front 24m of the insulation cover is completely closed, and the operation of the first to sixth rollers is gradually increased, with a speed of 0.5-1.2m / s.
[0038] (3) The diameter of the bar in this embodiment is Φ8.0 mm, and the chemical composition is C: 0.20-0.25%, Mn: 0.8-0.95%, Si: 0.15-0.30%, P: ≤0.013%, S: ≤0.020%, O≤0.0020%, [N]≤0.0045%, and the balance is Fe and unavoidable impurities. The hot-rolled structure is ferrite-troostite, the grain size is 9.0, the yield strength is 510-530 MPa, the tensile strength is 600-630 MPa, and the elongation is 1.25.
[0039] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0040] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A hot-rolled high-speed wire rod in-line wire calcining production process, characterized in that: The process includes: rolling, rapid cooling, low temperature wire laying, on-line wire sintering, coiling and PF line cooling: The rapid cooling step: the cooling capacity of the water tank is set to be not less than 350°C, the surface temperature of the rolled piece is controlled to be not less than 550°C, the wire drawing or coiling temperature is 600-650°C, and the temperature difference of the same batch of rolling is ±15°C.
2. The on-line sintering production process for hot-rolled high-speed wire rod according to claim 1, characterized in that: The rapid cooling means reducing the temperature of the rolled piece to the sorbite production temperature range of 600-650° C. within 3 seconds.
3. The on-line sintering production process for hot-rolled high-speed wire rod according to claim 1, characterized in that: The steps of on-line suturing are specifically as follows: The high-speed wire is kept warm on the air-cooling line for 30-150s after passing through the spinning machine or being coiled. The front 25-45m of the insulation cover is completely closed and the roller running speed is 0.2-2m / s. The insulation duration on the air-cooling roller is 30-150s to complete the transformation of the wire product from austenite to sorbite, and the sorbite content is ≥92%.
4. The on-line sintering production process for hot-rolled high-speed wire rod according to claim 1, characterized in that: The coiling and PF line cooling are completed in air cooling to below 80°C, which is convenient for inspection and sampling, cutting and storage.
5. The on-line sintering production process for hot-rolled high-speed wire rod according to claim 4, characterized in that: The wire coils shall continue to cool on the PF line for no less than 20 minutes after being wound.
6. The on-line sintering production process for hot-rolled high-speed wire rod according to claim 1, characterized in that: The rolling process is as follows: adopting two processes of austenite zone rolling and two-phase zone rolling, the final rolling deformation is controlled at 30-60%; the rolling temperature of the final rolling pass in the two-phase zone is Ar1-Ar3 or Ar1-Arcm, and the rolling temperature difference of the same batch is ±15°C; the rolling temperature of the final rolling pass in the austenite zone is Ar3-1000°C, and the rolling temperature difference of the same batch is ±15°C.
7. The on-line sintering production process for hot-rolled high-speed wire rod according to claim 1, characterized in that: The rapid cooling process adopts a multi-section annular venturi nozzle, 6-9 groups of which are placed in a closed box, and the outlet and inlet are water-sealed and air-sealed to prevent steam and water from being carried out of the water tank; 3-5 sets of such water tanks are provided, and the cooling capacity is not less than 350°C; a surface detection device is provided in the cooling zone to control the surface temperature of the rolled piece to be not less than 550°C, the wire drawing or coiling temperature is 600-650°C, and the temperature difference of the same batch of rolling is ±15°C.
Citation Information
Patent Citations
Method for producing good-quality high-carbon steel green rod for drawing
CN101327490A
Coil production method and production line thereof
CN105665442A
Controlled-rolling and controlled-cooling online sorbite process of stainless steel hot-rolled coiled plate
CN110283980A
15.9-grade annealing-free hot-rolled high-carbon vanadium-containing cold heading steel wire rod and manufacturing method thereof
CN118639123A
Cooling control method used for steels after hot rolled
CN1189400A