Preparation method of porous hard alloy bearing and porous hard alloy bearing
By adding resin to cemented carbide bearings to form pores, the problems of large wear of bearings at high temperatures and difficult lubricant management are solved, and the automatic management of lubricant and wear reduction are achieved.
Patent Information
- Application Number
- CN202411260417.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
AI Technical Summary
Carbide bearings wear heavily at high temperatures. Traditional methods such as improving surface finish and adding lubricant oil have problems with low operability and oil leakage.
By adding resin during the preparation of cemented carbide bearings, uniformly distributed pores are formed to absorb and release lubricating oil, the cumbersomeness of frequent refueling and the oil leakage problem is solved.
It realizes rapid absorption of lubricating oil in the initial wet state and releases it while working, reducing wear and improving the wear resistance and service life of the bearing.
Smart Images

Figure CN119076956A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cemented carbide production technology, and in particular to a preparation method of a porous cemented carbide bearing and a porous cemented carbide bearing. Background Art
[0002] With the modernization of the bearing field, various mechanical bearings have entered a new stage of development. Due to the complex and harsh working environment of bearings, the surface finish and internal structure of the bearings are very important for their performance. In the traditional fields of aviation, aerospace, and automotive parts, various new types of bearings are increasingly widely used. Cemented carbide is an alloy bearing made of hard compounds of refractory metals and bonding metals through powder metallurgy. It has the characteristics of high hardness, relatively good strength and toughness, and also has certain excellent properties such as heat resistance and corrosion resistance. Therefore, cemented carbide is an important bearing for the preparation of bearings.
[0003] In order to solve the problem of high working temperature and large wear of cemented carbide bearings, on the one hand, the wear is reduced by improving the surface finish of the bearing. The amount of wear reduced by this method is very small and almost negligible; on the other hand, the working temperature and wear are reduced by adding lubricating oil to the working environment of the bearing. This method is not easy to operate, and the oil needs to be changed frequently and there is a risk of oil leakage.
[0004] The above contents are only used to assist in understanding the technical solution of the present invention and do not constitute an admission that the above contents are prior art. Summary of the invention
[0005] The main purpose of the present invention is to solve the technical problems described in the background technology.
[0006] To achieve the above objectives, in a first aspect, the present invention provides a method for preparing a porous cemented carbide bearing, the method comprising:
[0007] obtaining a first mixture, the first mixture comprising cobalt and tungsten carbide;
[0008] Wet-grinding a wet-grinding medium, a forming agent, and the first mixture to obtain a second mixture;
[0009] The second mixture is subjected to a drying and granulation operation to obtain a third mixture;
[0010] obtaining a resin, and mixing the resin into the third mixture to obtain a fourth mixture;
[0011] The fourth mixture is pressed into a preset shape and sintered to remove the resin to obtain a porous cemented carbide bearing.
[0012] In one embodiment, the step of pressing the fourth mixture into a preset shape and sintering to remove the resin to obtain a porous cemented carbide bearing comprises:
[0013] Pressing the fourth mixture into a preset shape to obtain a bearing pressed embryo;
[0014] placing the bearing compact into a sintering furnace and maintaining the compact at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product;
[0015] Maintaining the first semi-finished product at a second temperature for a second period of time to obtain a second semi-finished product;
[0016] Maintaining the second semi-finished product at a third temperature for a third period of time to obtain a third semi-finished product;
[0017] The third semi-finished product is quickly cooled to room temperature to obtain the porous cemented carbide bearing.
[0018] In one embodiment, the step of placing the green compact in a sintering furnace and maintaining the green compact at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product comprises:
[0019] placing the bearing compact into a sintering furnace, heating the sintering furnace to a preset temperature and maintaining it for a fourth time period to remove the resin;
[0020] Continue to raise the temperature of the sintering furnace from the preset temperature to the first temperature and maintain it for a fifth time period to remove the forming agent to obtain a first semi-finished product, wherein the sum of the fourth time period and the fifth time period is equal to the first time period
[0021] In one embodiment, the step of placing the bearing compact into a sintering furnace and maintaining it at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product is replaced by:
[0022] Put the bearing compact into a graphite boat painted with paint, and put the graphite boat into a sintering furnace;
[0023] A preset flow rate of hydrogen is introduced into the sintering furnace, and the sintering furnace is maintained at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product.
[0024] In one embodiment, the first temperature is 380°C, the first time period is 5 hours, the second temperature is 1250°C, the second time period is 1 hour, the third temperature ranges from 1410°C to 1450°C, and the third time period is 1 hour.
[0025] In one embodiment, the step of drying the second mixture to obtain the third mixture is replaced by:
[0026] The third mixture is dried and granulated in a spray drying tower to obtain a third mixture, wherein the inlet temperature at the top of the spray drying tower is 160°C-240°C, the outlet temperature at the bottom of the tower is 80°C-110°C, and the internal pressure of the drying tower is 1.5kpa-2.0kpa.
[0027] In one embodiment, the cobalt has a Fisher grain size of less than 1 μm, the tungsten carbide has a grain size of 1 μm-3 μm and a carbon content of 6.12%-6.15%.
[0028] In one embodiment, the wet grinding medium is anhydrous ethanol with a concentration of not less than 98%, the molding agent includes paraffin and oleic acid, and the resin is bisphenol A.
[0029] In one embodiment, the cobalt accounts for 6%-10% of the weight of the first mixture, 0.35 L of anhydrous ethanol is configured per kilogram of the first mixture, the weight of the paraffin is 2%-3% of the weight of the first mixture, the weight of the oleic acid is 0.1%-0.2% of the weight of the paraffin, the weight of the resin is 2%-10% of the weight of the third mixture, and the diameter of the resin is 10μm-50μm.
[0030] In a second aspect, the present invention provides a porous cemented carbide bearing, which is prepared by any preparation method in the first aspect, and is characterized in that the porous cemented carbide bearing has evenly distributed pores, and the diameter of the pores is 10μm-50μm.
[0031] The present invention adds resin during the preparation of the porous cemented carbide bearing so that the prepared cemented carbide has uniformly distributed pores, can quickly absorb lubricating oil into the pores in the initial wet working state, and can release the lubricating oil in the pores while working in subsequent work, thereby eliminating the tediousness of frequently adding lubricating oil and solving the problem of bearing oil leakage. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 Schematic diagram of a process for preparing a porous cemented carbide bearing in one embodiment of the present invention;
[0034] Figure 2 Schematic diagram of a process for preparing a porous cemented carbide bearing in one embodiment of the present invention;
[0035] Figure 3 Schematic diagram of a process for preparing a porous cemented carbide bearing in one embodiment of the present invention;
[0036] Figure 4 Schematic diagram of a process for preparing a porous cemented carbide bearing in one embodiment of the present invention;
[0037] Figure 5 Schematic diagram of the surface state (a) and the internal state (b) of a porous cemented carbide bearing in one embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to better understand the above technical solution, exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.
[0039] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0040] It should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the coordinate system shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0041] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0042] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0043] The present invention provides a method for preparing a porous cemented carbide bearing. Figure 1 In one embodiment, the preparation method comprises:
[0044] S110, obtaining a first mixture, wherein the first mixture includes cobalt and tungsten carbide;
[0045] Among them, cobalt and tungsten carbide are both in powder form. Cobalt (Co) is a metal element, which is often used in the formulation of cemented carbide as a binder for tungsten carbide (WC) powder. Cobalt has good toughness and plasticity, which can increase the strength and impact resistance of cemented carbide. Tungsten carbide (WC) is a compound synthesized using two elements, tungsten and carbon. It has extremely high hardness, wear resistance and high melting point.
[0046] S120, wet-grinding a wet-grinding medium, a forming agent, and the first mixture to obtain a second mixture;
[0047] Specifically, the prepared first mixture, wet grinding medium, and forming agent are added into a wet grinder together, and the wet grinding time is set to ensure that the first mixture, wet grinding medium, and forming agent are fully and evenly mixed.
[0048] S130, performing a drying and granulation operation on the second mixture to obtain a third mixture;
[0049] Specifically, the wet-milled second mixture is dried and granulated to obtain a granular third mixture.
[0050] S140, obtaining a resin, and mixing the resin into the third mixture to obtain a fourth mixture;
[0051] Wherein, the resin is made of bisphenol A, and its chemical formula is C 15 H 16 O2.
[0052] Specifically, obtain a proper amount of resin with a preset diameter, mix the third mixture with a proper amount of resin, and use a stirrer or other tool to stir them to ensure that they are evenly mixed until the two are fully mixed.
[0053] S150, pressing the fourth mixture into a preset shape and sintering the mixture to remove the resin to obtain a porous cemented carbide bearing.
[0054] Specifically, a press is used to form the fourth mixture into a preset shape, which is the shape of the required bearing, and the mixture is sintered. During the sintering process, the resin and the molding agent are removed, and after the sintering is completed, a porous cemented carbide bearing is obtained.
[0055] In this embodiment, resin is added during the preparation of the porous cemented carbide bearing, and the resin is completely volatilized during the sintering process so that pores corresponding to the shape of the resin are evenly distributed in the porous cemented carbide bearing (refer to Figure 5 , where black represents pores), the size of the pores in the porous carbide bearing can be controlled by controlling the diameter of the resin, and the porosity in the porous carbide bearing can be controlled by controlling the amount of resin used. The pores can quickly absorb lubricating oil in the bearing made of porous carbide under the initial working state, and can release the lubricating oil in the pores while working in subsequent work, eliminating the tediousness of frequent addition of lubricating oil and solving the problem of bearing oil leakage.
[0056] In one embodiment, referring to Figure 2 S150, the step of pressing the fourth mixture into a preset shape and sintering to remove the resin to obtain a porous cemented carbide bearing comprises:
[0057] S151, pressing the fourth mixture into a preset shape to obtain a bearing compact;
[0058] Specifically, the fourth mixture is pressed into a bearing blank of a desired shape using a press or other equipment, and the bearing blank is ensured to be filled into a mold to form a preliminary shape of the bearing.
[0059] S152, placing the bearing compact into a sintering furnace, and maintaining the bearing compact at a first temperature for a first period of time to remove the resin and the molding agent, thereby obtaining a first semi-finished product;
[0060] Among them, the sintering furnace is an integrated "dewaxing-sintering" furnace capable of high-pressure sintering.
[0061] Specifically, the compact is placed in a "dewaxing-sintering" integrated furnace, and the integrated furnace is controlled to heat up to a first temperature and keep the temperature for a first period of time to remove the molding agent and the mixed resin.
[0062] S153, maintaining the first semi-finished product at a second temperature for a second period of time to obtain a second semi-finished product;
[0063] Specifically, the vacuum environment in the sintering furnace should be maintained in this step.
[0064] S154, maintaining the second semi-finished product at a third temperature for a third period of time to obtain a third semi-finished product;
[0065] Among them, the vacuum degree in the integrated furnace in this step is 10Pa.
[0066] S155, rapidly cooling the third semi-finished product to room temperature to obtain the porous cemented carbide bearing.
[0067] In this embodiment, different temperatures and holding times can be adjusted according to requirements to prepare porous cemented carbide bearings with different weights and performances.
[0068] In one embodiment, referring to Figure 4 S152, placing the bearing compact into a sintering furnace and maintaining it at a first temperature for a first period of time to remove the resin and the molding agent, and obtaining a first semi-finished product comprises:
[0069] S1521, placing the bearing compact into the sintering furnace, heating the sintering furnace to a preset temperature and maintaining it for a fourth time period to remove the resin;
[0070] Specifically, the sintering furnace is heated to a preset temperature and maintained for a fourth period of time in order to remove the resin. The temperature for resin cracking is about 180 degrees, and the preset temperature is set according to the temperature for resin cracking.
[0071] S1521, continue to heat the sintering furnace from the preset temperature to the first temperature and maintain it for a fifth time period to completely remove the resin and the molding agent to obtain a first semi-finished product, wherein the sum of the fourth time period and the fifth time period is equal to the first time period.
[0072] The molding agent may be paraffin or PEG (polyethylene glycol). When the molding agent is paraffin, since paraffin is insoluble in ethanol, oleic acid should be added simultaneously to make the paraffin and other substances evenly mixed.
[0073] Specifically, the pyrolysis temperatures of paraffin and PEG are both around 300 degrees. The first temperature is set according to the pyrolysis temperatures of molding agents such as paraffin or PEG. A small amount of the molding agent will be removed below the pyrolysis temperature.
[0074] In one embodiment, referring to Figure 3 , S152, placing the bearing compact into a sintering furnace, maintaining it at a first temperature for a first period of time to remove the resin and the molding agent, and the step of obtaining a first semi-finished product is replaced by:
[0075] S1521, placing the bearing compact into a graphite boat coated with paint, and placing the graphite boat into a sintering furnace;
[0076] Among them, the main formula of the coating includes: carbon black, Tween, distilled water or PEG, etc., which can isolate the product and the graphite boat to prevent sticking to the boat and make the product have better sintering performance.
[0077] Specifically, the coating is applied on a graphite boat, and the compact is loaded into the graphite boat and placed in a sintering furnace.
[0078] S1522, introducing a preset flow rate of hydrogen into the sintering furnace, and maintaining the sintering furnace at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product.
[0079] In addition to hydrogen, other gases such as helium and argon can also be used. From room temperature to the first temperature, hydrogen is used to discharge the cracked resin and molding agent out of the furnace, and an open flame is ignited outside the furnace to burn.
[0080] For example, the preset flow rate is 3m 3 / h-5m 3 / h, the first temperature is 380°C, and the first time period is 5 hours.
[0081] In one embodiment, referring to Figure 1-3 The first temperature is 380°C, the first time period is 5 hours, the second temperature is 1250°C, the second time period is 1 hour, the third temperature ranges from 1410°C to 1450°C, and the third time period is 1 hour.
[0082] Specifically, in this embodiment, the sintering furnace is 3m 3 / h-5m 3 / h of hydrogen and the temperature is raised to 380°C, and the temperature is kept for 1 hour to remove the molding agent and resin to obtain a first semi-finished product; then the temperature is raised to 1250°C in a vacuum atmosphere and the temperature is kept for 1 hour to obtain a second semi-finished product; the temperature is further raised to 1410°C-1450°C, and the vacuum degree is 10Pa and sintered for 1 hour to obtain a third semi-finished product; after sintering, it is quickly cooled to room temperature to obtain the porous cemented carbide bearing.
[0083] In one embodiment, the step of drying the second mixture to obtain the third mixture is replaced by:
[0084] The third mixture is dried and granulated in a spray drying tower to obtain a third mixture, wherein the inlet temperature at the top of the spray drying tower is 160°C-240°C, the outlet temperature at the bottom of the tower is 80°C-110°C, and the internal pressure of the drying tower is 1.5kpa-2.0kpa.
[0085] Among them, the spray drying tower is an industrial equipment used to dry liquid or slurry materials into powder or particles through spray and hot air. It can atomize the liquid or slurry into fine droplets through a nozzle, and then quickly evaporate the water in the droplets under the action of hot air, finally forming dry powder or particles.
[0086] In this embodiment, a spray drying tower is used, the second mixture is dried quickly, the surface area of the liquid material is greatly increased after atomization, 95%-98% of the water can be evaporated instantly in the hot air flow, and the drying time is only a few seconds. The material has good uniformity and fluidity, the product purity is high, and the quality is good; the production process is simplified, and the operation and control are convenient.
[0087] In one embodiment, referring to Figure 1-3 The wet grinding medium, the molding agent and the first mixture are wet-milled in a wet mill. The ball mill in the wet mill is a YG8 carbide ball mill with a diameter of φ5.5mm×17mm-φ10.5mm×17mm. The rotation speed of the ball mill in the wet mill is 36-50r / min.
[0088] In this embodiment, wet grinding is to add the prepared raw materials, wet grinding media and forming agent into a wet grinder and mix them together, so that the raw materials of each component can be fully mixed evenly.
[0089] In one embodiment, referring to Figure 1-3 The cobalt has a Fisher grain size of less than 1 μm, the tungsten carbide has a grain size of 1 μm-3 μm and a carbon content of 6.12%-6.15%.
[0090] In one embodiment, referring to Figure 1-3 The wet grinding medium is anhydrous ethanol with a concentration of not less than 98%, the molding agent includes paraffin and oleic acid, and the resin is bisphenol A.
[0091] Among them, paraffin is used as a molding agent in the preparation process of cemented carbide. Paraffin has good lubricating properties. It is mainly used to improve the fluidity and plasticity of the powder during the pressing process, play the role of lubrication, bonding and filling, and make the powder easier to press into a blank with a certain shape and strength. Since paraffin is insoluble in anhydrous ethanol as a wet grinding medium, oleic acid is added to mix the paraffin and other substances. After removing the paraffin, the blank can be sintered at high temperature to form a high-density, high-performance cemented carbide product.
[0092] In one embodiment, referring to Figure 1-3The cobalt accounts for 6%-10% of the weight of the first mixture, 0.35L of anhydrous ethanol is configured per kilogram of the first mixture, the weight of the paraffin is 2%-3% of the weight of the first mixture, the weight of the oleic acid is 0.1%-0.2% of the weight of the paraffin, the weight of the resin is 2%-10% of the weight of the third mixture, and the diameter of the resin is 10μm-50μm.
[0093] Second, refer to Figure 5 The present invention provides a porous cemented carbide bearing, which is prepared by any preparation method in the first aspect, and is characterized in that the porous cemented carbide bearing has evenly distributed pores, and the diameter of the pores is 10μm-50μm.
[0094] In this embodiment, by using a porous carbide bearing with uniformly distributed pores, the bearing can quickly absorb lubricating oil into the pores of the bearing itself in the initial wet working state, and can release the lubricating oil in the pores while working in subsequent work, eliminating the tediousness of frequently adding lubricating oil and solving the problem of bearing oil leakage.
[0095] In one embodiment, resins with diameters of 50 μm, 30 μm, and 10 μm were obtained, and three porous cemented carbide bearings were made according to the preparation method described in the first aspect based on these resins. The porosity (Vol%), hardness (HRA) and friction coefficient (μ) of the three cemented carbides in the wet state were measured using a porosity measuring device, a hardness measuring device, and a wet friction coefficient testing device. The measurement results are shown in the following table:
[0096] Resin diameter Porosity Vol% Hardness HRA Friction coefficient in wet state (μ) 50μm 30 67 0.05 30μm 20 78 0.18 10μm 10 85 0.32 0μm 0 92 0.46
[0097] It is important to understand that cemented carbide is widely used in various industrial fields, including cutting tools, molds, and bearings, due to its high hardness and excellent wear resistance. Bearings need to have good wear resistance and anti-friction properties. The smaller the friction coefficient in the wet state, the smaller the friction of the bearing and the better the wear resistance of the bearing.
[0098] According to the above table, it can be seen that the porous carbide bearings produced in this application have a very small friction coefficient in a wet state, and the greater the porosity of the carbide bearings, the smaller the friction coefficient, that is, the performance of the porous carbide bearings can well meet the requirements for manufacturing bearings.
[0099] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a porous cemented carbide bearing, characterized in that: The preparation method comprises: obtaining a first mixture, the first mixture comprising cobalt and tungsten carbide; Wet-grinding a wet-grinding medium, a forming agent, and the first mixture to obtain a second mixture; The second mixture is subjected to a drying and granulation operation to obtain a third mixture; obtaining a resin, and mixing the resin into the third mixture to obtain a fourth mixture; The fourth mixture is pressed into a preset shape and sintered to remove the resin to obtain a porous cemented carbide bearing.
2. The method for preparing a porous cemented carbide bearing according to claim 1, characterized in that: The step of pressing the fourth mixture into a preset shape and sintering to remove the resin to obtain a porous cemented carbide bearing comprises: Pressing the fourth mixture into a preset shape to obtain a bearing pressed embryo; placing the bearing compact into the sintering furnace and maintaining it at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product; Maintaining the first semi-finished product at a second temperature for a second period of time to obtain a second semi-finished product; Maintaining the second semi-finished product at a third temperature for a third period of time to obtain a third semi-finished product; The third semi-finished product is quickly cooled to room temperature to obtain the porous cemented carbide bearing.
3. The method for preparing a porous cemented carbide bearing according to claim 2, wherein the step of placing the bearing compact into a sintering furnace and maintaining the bearing compact at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product comprises: placing the bearing compact into the sintering furnace, heating the sintering furnace to a preset temperature and maintaining it for a fourth time period to remove the resin; The sintering furnace is continuously heated from the preset temperature to the first temperature and maintained for a fifth time period to remove the forming agent and obtain a first semi-finished product, wherein the sum of the fourth time period and the fifth time period is equal to the first time period.
4. The method for preparing a porous cemented carbide bearing according to claim 2, wherein the step of placing the bearing compact into a sintering furnace and maintaining the bearing compact at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product is replaced by: Put the bearing compact into a graphite boat painted with paint, and put the graphite boat into the sintering furnace; A preset flow rate of hydrogen is introduced into the sintering furnace, and the sintering furnace is maintained at a first temperature for a first period of time to remove the resin and the molding agent to obtain a first semi-finished product.
5. The method for preparing a porous cemented carbide bearing according to claim 2, characterized in that: The first temperature is 380° C., the first time period is 5 hours, the second temperature is 1250° C., the second time period is 1 hour, the third temperature ranges from 1410° C. to 1450° C., and the third time period is 1 hour.
6. The method for preparing a porous cemented carbide bearing according to claim 1, characterized in that: The step of drying the second mixture to obtain the third mixture is replaced by: The third mixture is dried and granulated in a spray drying tower to obtain a third mixture, wherein the inlet temperature at the top of the spray drying tower is 160°C-240°C, the outlet temperature at the bottom of the tower is 80°C-110°C, and the internal pressure of the drying tower is 1.5kpa-2.0kpa.
7. The method for preparing a porous cemented carbide bearing according to claim 1, characterized in that: The cobalt has a Fisher grain size of less than 1 μm, the tungsten carbide has a grain size of 1 μm-3 μm and a carbon content of 6.12%-6.15%.
8. The method for preparing a porous cemented carbide bearing according to claim 1, characterized in that: The wet grinding medium is anhydrous ethanol with a concentration of not less than 98%, the molding agent includes paraffin and oleic acid, and the resin is made of bisphenol A.
9. The method for preparing a porous cemented carbide bearing according to claim 8, characterized in that: The cobalt accounts for 6%-10% of the weight of the first mixture, 0.35L of anhydrous ethanol is configured per kilogram of the first mixture, the weight of the paraffin is 2%-3% of the weight of the first mixture, the weight of the oleic acid is 0.1%-0.2% of the weight of the paraffin, the weight of the resin is 2%-10% of the weight of the third mixture, and the diameter of the resin is 10μm-50μm.
10. A porous cemented carbide bearing, which is prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The porous cemented carbide bearing has evenly distributed pores, and the diameter of the pores is 10 μm-50 μm.