Lead-free solder for narrow-spacing and high-density packaging as well as preparation method and application of lead-free solder

A lead-free solder with a specific composition and preparation method enhances thermal cycle reliability and high-temperature shock resistance for narrow pitch, high-density packaging by using Ag, Cu, Sb, Mg, and B alloys, addressing solder joint failures in high-frequency environments.

CN119077212APending Publication Date: 2024-12-06BEIJING COMPO ADVANCED TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411258275.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing solder alloys used in narrow pitch, high-density packaging face issues with accelerated atomic migration, thermal fatigue, and solder joint failure due to high frequency and temperature changes, leading to reliability concerns.

Method used

A lead-free solder composition comprising Ag, Cu, Sb, Mg, Ti, and B, with specific mass percentages, and a preparation method involving induction melting and alloying to create a fine structure with improved thermal cycle reliability.

Benefits of technology

The lead-free solder achieves higher high-temperature shock resistance and thermal cycle reliability, addressing the reliability issues in narrow pitch, high-density packaging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077212A_ABST
    Figure CN119077212A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lead-free solder, and particularly relates to lead-free solder for narrow-spacing and high-density packaging and a preparation method and application of the lead-free solder. The lead-free solder for narrow-pitch and high-density packaging is prepared from the following elements in percentage by mass: 0.05 wt.% to 0.4 wt.% of Ag, 0.2 wt.% to 0.8 wt.% of Cu, 0.1 wt.% to 2.0 wt.% of Sb, 0.01 wt.% to 2.0 wt.% of Mg, 0.02 wt.% to 3.5 wt.% of Ti, 0.002 wt.% to 1.5 wt.% of B and the balance of Sn and inevitable impurities. The lead-free solder does not contain magnetic elements such as Fe, Co and Ni and radioactive elements such as Bi and Pb, the structure is fine, components are uniform, welding spots of the lead-free solder have higher high-temperature impact resistance and thermal cycle reliability, and the lead-free solder can be used in the field of 5G communication narrow-spacing and high-density packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lead-free solders, and in particular relates to a lead-free solder for narrow spacing and high-density packaging, and a preparation method and application thereof. Background Art

[0002] In recent years, industries such as high-speed communication networks, the Internet of Things, cloud computing, and artificial intelligence based on 5G communications have developed rapidly. A large number of 5G application scenarios are in the high-frequency bands of 15G and above, and the characteristics of the service materials at this time will have a significant impact on the terminal signal. As a key material in the manufacturing process of 5G communication products, solder alloys play the role of triple interconnection of electricity, heat, and force. In the field of narrow pitch and high-density packaging, in the multi-physical field coupling environment created by high frequency and high current inclusions, the traditional Sn-Ag-Cu solder alloys, on the one hand, are under the action of the thermoelectric coupling field. The atomic migration rate is accelerated, and the cathode atoms of the solder joints continue to diffuse to the anode, generating large tensile stress around the cathode; on the other hand, with the drastic change in temperature, the solder joints face stronger thermal fatigue damage, microcracks quickly nucleate and expand, and eventually lead to solder joint failure.

[0003] Therefore, more stringent technical requirements are placed on the reliability of solder alloys used in narrow pitch, high-density packaging, and existing solder alloys still need to be improved. Summary of the invention

[0004] The main purpose of the present invention is to provide a lead-free solder for narrow pitch and high density packaging and its preparation method and use. The lead-free solder in the present invention does not contain magnetic elements such as Fe, Co and Ni and radioactive elements such as Bi and Pb, has a fine structure and uniform composition, and its solder joints have higher high temperature shock resistance and thermal cycle reliability.

[0005] In order to achieve the above objectives, the present invention provides the following technical solutions.

[0006] In a first aspect, the present invention provides a lead-free solder for narrow pitch and high density packaging. The lead-free solder comprises the following elements in mass percentage: Ag 0.05wt.% to 0.4wt.%, Cu 0.2wt.% to 0.8wt.%, Sb 0.1wt.% to 2.0wt.%, Mg 0.01wt.% to 2.0wt.%, Ti 0.02wt.% to 3.5wt.%, B 0.002wt.% to 1.5wt.%, and the remainder is Sn and unavoidable impurities.

[0007] In some embodiments of the present invention, the mass percentage of the Ag element is 0.1wt.% to 0.4wt.%; and / or,

[0008] The mass percentage of the Cu element is 0.3wt.% to 0.8wt.%; and / or,

[0009] The mass percentage of the Sb element is 0.2wt.% to 1.8wt.%; and / or,

[0010] The mass percentage of the Mg element is 0.1wt.% to 1.6wt.%; and / or,

[0011] The mass percentage of the Ti element is 0.05wt.% to 2.5wt.%; and / or,

[0012] The mass percentage of the B element is 0.1 wt.% to 1.1 wt.%.

[0013] The second aspect of the present invention provides a method for preparing the lead-free solder described in the first aspect. The preparation method comprises the following steps: using induction melting method to prepare Sn-Cu, Sn-Ag, Sn-Sb, Sn-Cu-Ti-B master alloys respectively; mixing and melting pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy according to the required ratio to obtain alloy melt; and keeping the alloy melt at 450℃~550℃ for a period of time, adding the Sn-Cu-Ti-B master alloy, and fully melting to obtain a mixed melt; adding magnesium melt to the mixed melt, keeping it warm and casting to obtain a lead-free solder ingot.

[0014] In some embodiments of the present invention, the preparation of the Sn-Cu-Ti-B master alloy includes: preparing a Sn-Ti master alloy and a Cu-B master alloy respectively by an induction melting method; mixing and melting the Sn-Cu master alloy and the Cu-B master alloy according to a required ratio to obtain a Sn-Cu-B master alloy; mixing and melting the Sn-Ti master alloy and the Sn-Cu-B master alloy according to a required ratio to obtain the Sn-Cu-Ti-B master alloy.

[0015] In some embodiments of the present invention, the smelting process of the Sn-Cu-B master alloy includes: melting the Sn-Cu master alloy and then adding the Cu-B master alloy, and stirring the mixture evenly.

[0016] In some embodiments of the present invention, the preparation process of the magnesium melt includes: preheating a smelting furnace at a temperature of 100°C to 300°C for 1h to 3h; adding metallic magnesium, heating it to 650°C to 750°C under a protective atmosphere, and keeping it warm until it is completely melted.

[0017] In some embodiments of the present invention, the temperature for mixed melting of pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy is 500°C to 600°C.

[0018] In some embodiments of the present invention, the alloy melt is kept at a temperature of 450° C. to 550° C. for 20 min to 60 min.

[0019] In some embodiments of the present invention, the holding time from adding magnesium melt to the mixed melt to before pouring is 5 min to 30 min.

[0020] In some embodiments of the present invention, the preparation method further comprises converting the lead-free solder ingot into at least one of a paste, a tape, a foil, a sheet, a wire or a powder.

[0021] The third aspect of the present invention provides a use of the lead-free solder described in the first aspect or the lead-free solder prepared by the preparation method described in the second aspect as solder for 5G communication electronic devices.

[0022] Compared with the prior art, the present invention achieves the following technical effects:

[0023] The lead-free solder alloy in the present invention has a fine structure and uniform composition, and its solder joints have higher thermal shock and thermal cycle reliability, and can be used in the field of narrow spacing and high-density packaging of 5G communications.

[0024] In the low-cost lead-free solder alloy of the present invention, part of the added Sb element is dissolved in the matrix to generate a strain field, which effectively hinders the movement of dislocations and improves the strength and impact resistance of the alloy; part of it exists in the matrix in the form of Sn-Sb intermetallic compounds, which plays a role in refining the structure; and part of it exists in the interface formed by the solder alloy and the Cu substrate, which reduces the diffusion rate of Cu in Sn and inhibits the growth of the Cu-Sn intermetallic compound layer.

[0025] In the low-cost lead-free solder alloy of the present invention, the addition of Mg element can form a primary phase containing Mg at the interface, which serves as the nucleation center of the Cu6Sn5 phase and refines the Cu-Sn intermetallic compound layer.

[0026] In the low-cost lead-free solder alloy of the present invention, Ti and B elements are simultaneously introduced in the form of an intermediate alloy, which can generate TiB2 phase and Sn3Ti2 phase in situ in the solder alloy matrix on the one hand, and on the other hand, some B single substance can be dispersed in the matrix, and these second phase particles can reduce the supercooling degree of nucleation, thereby achieving the purpose of refining the organization, and at the same time, a small amount of B elements concentrated at the interface of the solder joint can hinder the diffusion of Cu into Sn. The refinement of the organization can improve the strength of the solder, and the refinement of the Cu-Sn intermetallic compound layer and the inhibition of diffusion between Cu-Sn can greatly improve the high-cycle impact resistance and thermal cycle reliability of the solder alloy.

[0027] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:

[0029] Figure 1 The microstructure diagram of the solder prepared in Example 1;

[0030] Figure 2 Schematic diagram of solder joint shear strength test. DETAILED DESCRIPTION

[0031] The exemplary embodiments of the present invention will be described in more detail below with reference to specific embodiments. It should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" in the specification and claims of the present invention and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0033] In the description of the embodiments of the present invention, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present invention, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0034] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0035] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this document generally indicates that the associated objects before and after are in an "or" relationship.

[0036] In the description of the embodiments of the present invention, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0037] At present, most of the mainstream high-reliability alloys in the world are designed for automotive circuits, such as the Innolot alloy developed by Alpha in the United States, the M794 alloy developed by Senju Metal Industries Co., Ltd. in Japan, and the REL22 alloy developed by AIM. Tm Alloy and LSP alloy of Harima Chemical Group. These solder alloys mainly improve reliability by microalloying. The microalloying mechanism mainly includes: introducing elements that are not combined with matrix elements but have solid solution strengthening and dispersion strengthening effects on the matrix; introducing elements that combine with the main element Sn, thereby reducing the nucleation supercooling of β-Sn and achieving fine grain strengthening; introducing elements that combine with the main element Sn and the substrate Cu to inhibit the growth of intermetallic compounds at the interface during aging. However, in order to obtain higher welding strength, creep resistance and reliability under non-extreme thermal cycle conditions, the above solder alloys often contain higher Ag elements, which invisibly increases the cost of materials. In addition, among the commonly used microalloying elements, the magnetic permeability of Fe, Co and Ni will change nonlinearly with the change of magnetic field, which is easy to cause two or more signals to generate strong interference signals, and finally interfere with the communication system; elements such as Bi are naturally radioactive and can release α particles with strong ionization ability, which increases the probability of soft errors in devices serving in the field of narrow spacing and high-density packaging, and then the data loss and function interruption of electronic equipment will occur.

[0038] To this end, the present invention provides a lead-free solder for narrow pitch and high density packaging and a preparation method thereof. The lead-free solder can be used as a solder for narrow pitch and high density packaging, and the lead-free solder contains tin, silver, copper, antimony, magnesium, titanium and boron elements, but does not contain magnetic elements such as Fe, Co and Ni and radioactive elements such as Bi and Pb, has a fine structure and uniform composition, and its solder joints have higher high temperature shock resistance and thermal cycle reliability.

[0039] The lead-free solder for narrow pitch and high density packaging in the present invention comprises the following elements in mass percentage: Ag 0.05wt.% to 0.4wt.%, Cu 0.2wt.% to 0.8wt.%, Sb 0.1wt.% to 2.0wt.%, Mg 0.01wt.% to 2.0wt.%, Ti 0.02wt.% to 3.5wt.%, B 0.002wt.% to 1.5wt.%, and the rest are Sn and unavoidable impurities.

[0040] In some embodiments of the present invention, the mass percentage of the Ag element is 0.1 wt.% to 0.4 wt.%.

[0041] The mass percentage of the Ag element provided by the present invention can be one of 0.05wt.%, 0.06wt.%, 0.07wt.%, 0.08wt.%, 0.09wt.%, 0.1wt.%, 0.12wt.%, 0.14wt.%, 0.15wt.%, 0.16wt.%, 0.18wt.%, 0.2wt.%, 0.22wt.%, 0.24wt.%, 0.25wt.%, 0.26wt.%, 0.28wt.%, 0.3wt.%, 0.32wt.%, 0.34wt.%, 0.35wt.%, 0.36wt.%, 0.38wt.%, 0.4wt.% or any value that meets the above range.

[0042] In some embodiments of the present invention, the mass percentage of Cu element is 0.3 wt.% to 0.8 wt.%.

[0043] The mass percentage of the Cu element provided by the present invention can be 0.2wt.%, 0.22wt.%, 0.24wt.%, 0.25wt.%, 0.26wt.%, 0.28wt.%, 0.3wt.%, 0.32wt.%, 0.34wt.%, 0.35wt.%, 0.36wt.%, 0.38wt.%, 0.4wt.%, 0.42wt.%, 0.44wt.%, 0.46wt.%, 0.48wt.%, 0.5wt.% %, 0.52wt.%, 0.54wt.%, 0.55wt.%, 0.56wt.%, 0.58wt.%, 0.6wt.%, 0.62wt.%, 0.64wt.%, 0.65wt.%, 0.66wt.%, 0.68wt.%, 0.7wt.%, 0.72wt.%, 0.74wt.%, 0.75wt.%, 0.76wt.%, 0.78wt.%, 0.8wt.% or any value that meets the above range.

[0044] In some embodiments of the present invention, the mass percentage of the Sb element is 0.2 wt.% to 1.8 wt.%.

[0045] The mass percentage of the Sb element provided by the present invention can be one of 0.1wt.%, 0.2wt.%, 0.3wt.%, 0.4wt.%, 0.5wt.%, 0.6wt.%, 0.7wt.%, 0.8wt.%, 0.9wt.%, 1.0wt.%, 1.1wt.%, 1.2wt.%, 1.3wt.%, 1.4wt.%, 1.5wt.%, 1.6wt.%, 1.7wt.%, 1.8wt.%, 1.9wt.%, 2.0wt.% or any value that meets the above range.

[0046] In some embodiments of the present invention, the mass percentage of Mg element is 0.1 wt.% to 1.6 wt.%.

[0047] The mass percentage of the Mg element provided by the present invention can be one of 0.01wt.%, 0.02wt.%, 0.04wt.%, 0.06wt.%, 0.08wt.%, 0.1wt.%, 0.2wt.%, 0.3wt.%, 0.4wt.%, 0.5wt.%, 0.6wt.%, 0.7wt.%, 0.8wt.%, 0.9wt.%, 1.0wt.%, 1.2wt.%, 1.4wt.%, 1.6wt.%, 1.8wt.%, 2.0wt.% or any value that meets the above range.

[0048] In some embodiments of the present invention, the mass percentage of the Ti element is 0.05 wt.% to 2.5 wt.%.

[0049] The mass percentage of the Ti element provided by the present invention can be one of 0.02wt.%, 0.03wt.%, 0.04wt.%, 0.05wt.%, 0.06wt.%, 0.08wt.%, 0.1wt.%, 0.2wt.%, 0.4wt.%, 0.5wt.%, 0.6wt.%, 0.8wt.%, 1.0wt.%, 1.2wt.%, 1.3wt.%, 1.4wt.%, 1.5wt.%, 1.6wt.%, 1.8wt.%, 2.0wt.%, 2.2wt.%, 2.4wt.%, 2.5wt.%, 2.6wt.%, 2.8wt.%, 3.0wt.%, 3.2wt.%, 3.5wt.% or any value that meets the above range.

[0050] In some embodiments of the present invention, the mass percentage of element B is 0.1 wt.% to 1.1 wt.%.

[0051] The mass percentage of the B element provided by the present invention can be one of 0.002wt.%, 0.005wt.%, 0.006wt.%, 0.008wt.%, 0.01wt.%, 0.05wt.%, 0.08wt.%, 0.10wt.%, 0.20wt.%, 0.30wt.%, 0.40wt.%, 0.50wt.%, 0.60wt.%, 0.70wt.%, 0.80wt.%, 0.90wt.%, 1.0wt.%, 1.1wt.%, 1.2wt.%, 1.5wt.% or any value that meets the above range.

[0052] The invention also provides a method for preparing the lead-free solder for narrow spacing and high-density packaging, which is carried out according to the following steps.

[0053] (1) Preparation of intermediate alloy.

[0054] In the present invention, the induction melting method is adopted to prepare Sn-Cu master alloy, Sn-Ag master alloy, Sn-Sb master alloy, Sn-Ti master alloy and Cu-B master alloy respectively.

[0055] In some embodiments of the present invention, Sn-Cu master alloy and Cu-B master alloy are used as raw materials, the Sn-Cu master alloy and the Cu-B master alloy are mixed according to a required ratio, and induction melting method is used to melt to obtain Sn-Cu-B master alloy.

[0056] It is worth mentioning that the Sn-Cu-B master alloy must be prepared from Sn-Cu master alloy and Cu-B master alloy. The smelting process of the Sn-Cu-B master alloy includes: melting the Sn-Cu master alloy and then adding the Cu-B master alloy and stirring evenly.

[0057] In some embodiments of the present invention, Sn-Ti master alloy and Sn-Cu-B master alloy are mixed according to a desired ratio, and induction melting is used to melt to obtain Sn-Cu-Ti-B master alloy, thereby achieving the addition of Ti and B elements in lead-free solder.

[0058] (2) Pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy are added into a melting furnace A according to the required ratio and mixed and melted. A surface covering agent is added during the melting process to obtain an alloy melt.

[0059] In an embodiment of the present invention, the heating and melting temperature of the smelting furnace A is 500°C to 600°C, and the surface covering agent is added after the master alloy is completely melted. Exemplarily, the heating and melting temperature of the smelting furnace A can be one of 500°C, 520°C, 550°C, 580°C, 600°C, or any value that satisfies the above range.

[0060] In the embodiment of the present invention, the surface covering agent may be, but is not limited to, rosin, tin chloride, and the like.

[0061] (3) The above alloy melt is kept at 450° C. to 550° C. for 20 min to 60 min, Sn-Cu-Ti-B master alloy is added, and the temperature is kept until the alloy is fully melted to obtain a mixed melt.

[0062] In an embodiment of the present invention, the insulation temperature of the alloy melt may be one of 450° C., 500° C., 520° C., 550° C. or any value within the above range.

[0063] (4) Smelting of metallic magnesium.

[0064] In an embodiment of the present invention, the smelting furnace B is preheated at a temperature of 100° C. to 300° C. for 1 h to 3 h, metallic magnesium is added, and then a protective gas such as argon or helium is introduced, and the temperature is gradually raised to 650° C. to 750° C. and kept warm until it is completely melted to obtain a magnesium melt.

[0065] In an embodiment of the present invention, the melting temperature of the metal magnesium may be one of 650° C., 680° C., 700° C., 720° C., 750° C. or any value satisfying the above range.

[0066] In the embodiment of the present invention, the preheating temperature of the smelting furnace B can be one of 100° C., 150° C., 200° C., 250° C., 300° C. or any value within the above range. The preheating time can be one of 1 h, 1.5 h, 2 h, 2.5 h, 3 h or any value within the above range.

[0067] (5) The magnesium melt is transferred into the mixed melt in the smelting furnace A through a conveying pipe. After the melt is kept warm and the surface slag is removed, it is poured into a mold to obtain a solder alloy ingot.

[0068] In an embodiment of the present invention, the total holding time from the addition of the Sn-Cu-Ti-B master alloy to the full melting before pouring is 5 min to 30 min. Exemplarily, the total holding time can be one of 5 min, 10 min, 15 min, 20 min, 25 min or 30 min or any value satisfying the above range.

[0069] The lead-free solder provided in the present invention or the lead-free solder prepared by the above-mentioned preparation method is used as solder for 5G communication electronic devices.

[0070] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The experimental reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the raw materials, instruments and equipment used in the following examples, etc., can all be purchased on the market or can be obtained by existing methods; the amounts of the experimental reagents, unless otherwise specified, are the amounts of reagents used in conventional experimental operations; the experimental methods, unless otherwise specified, are all conventional methods.

[0071] Example 1

[0072] Provided are low-cost lead-free solder for narrow pitch and high-density packaging technology and a preparation method thereof. The alloy composition of the lead-free solder is: Ag 0.08wt.%, Cu 0.25wt.%, Sb 0.2wt.%, Mg 0.1wt.%, Ti 0.05wt.%, B 0.1wt.%, and the balance is Sn and unavoidable impurities.

[0073] The preparation method of the lead-free solder comprises the following steps:

[0074] (1) Sn-Cu master alloy, Sn-Ag master alloy, Sn-Sb master alloy, Sn-Ti master alloy and Cu-B master alloy were prepared by induction melting method.

[0075] (2) Using the Sn-Cu master alloy and the Cu-B master alloy in step (1) as raw materials, according to the required alloy ratio, an induction melting method is used to prepare a Sn-Cu-B master alloy. During the melting, the Sn-Cu master alloy is first melted and then the Cu-B master alloy is added and stirred evenly.

[0076] (3) According to the required alloy ratio, the Sn-Ti master alloy and the Sn-Cu-B master alloy are mixed and smelted to obtain the Sn-Cu-Ti-B master alloy.

[0077] (4) Pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy are added into a melting furnace A according to the required ratio, and mixed and melted to obtain alloy melt. The melting temperature is 500° C., and rosin is added after the master alloy is completely melted.

[0078] (5) The alloy melt in the furnace melt A is kept at 450° C. for 60 min, and the Sn-Cu-Ti-B master alloy is added and kept warm until it is fully melted to obtain a mixed melt.

[0079] (6) The smelting furnace B is preheated at 150°C for 3 h, and metallic Mg is added. Argon gas is introduced and the temperature is raised to 650°C. The temperature is kept until it is completely melted. Subsequently, the molten magnesium is transferred to the bottom of the mixed melt in the smelting furnace A through an infusion tube and kept warm for 5 min. After removing the surface oxide slag, the melt is poured into a mold to obtain a solder alloy ingot.

[0080] Example 2

[0081] Provided is a low-cost lead-free solder for narrow pitch, high-density packaging technology and a preparation method thereof. The preparation method is the same as that of Example 1, except that:

[0082] The alloy composition of the lead-free solder is: Ag 0.15wt.%, Cu 0.4wt.%, Sb 0.4wt.%, Mg 0.3wt.%, Ti 0.2wt.%, B 0.4wt.%, and the balance is Sn and inevitable impurities.

[0083] Example 3

[0084] Provided are a low-cost lead-free solder for narrow pitch and high-density packaging technology and a preparation method thereof. The alloy components of the lead-free solder are: Ag 0.2wt.%, Cu 0.5wt.%, Sb 0.8wt.%, Mg 0.5wt.%, Ti 0.5wt.%, B 0.2wt.%, and the remainder is Sn and unavoidable impurities.

[0085] The preparation method of the lead-free solder comprises the following steps:

[0086] (1) Sn-Cu master alloy, Sn-Ag master alloy, Sn-Sb master alloy, Sn-Ti master alloy and Cu-B master alloy were prepared by induction melting method.

[0087] (2) Using the Sn-Cu master alloy and the Cu-B master alloy in step (1) as raw materials, according to the required alloy ratio, an induction melting method is used to prepare a Sn-Cu-B master alloy. During the melting, the Sn-Cu master alloy is first melted and then the Cu-B master alloy is added and stirred evenly.

[0088] (3) According to the required alloy ratio, the Sn-Ti master alloy and the Sn-Cu-B master alloy are mixed and smelted to obtain the Sn-Cu-Ti-B master alloy.

[0089] (4) Pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy are added into a melting furnace A according to the required alloy ratio, and mixed and melted to obtain alloy melt. The melting temperature is 550° C., and rosin is added after the master alloy is completely melted.

[0090] (5) The alloy melt in the furnace melt A is kept at 500° C. for 45 min, and the Sn-Cu-Ti-B master alloy is added and kept warm until it is fully melted to obtain a mixed melt.

[0091] (6) The smelting furnace B is preheated at 200°C for 2 h, and metallic Mg is added. Argon gas is introduced and the temperature is raised to 720°C. The temperature is kept until the molten magnesium is completely melted. The molten magnesium is then transferred to the bottom of the mixed melt in the smelting furnace A through a liquid infusion tube and kept warm for 15 min. After removing the surface oxide slag, the melt is poured into a mold to obtain a solder alloy ingot.

[0092] Examples 4 to 6 respectively provide a low-cost lead-free solder for narrow pitch, high-density packaging and a preparation method thereof, wherein the preparation method of the lead-free solder in Examples 4 to 6 is the same as that in Example 3, the only difference being the alloy composition of the lead-free solder.

[0093] The alloy composition of the lead-free solder in Example 4 is: Ag 0.25wt.%, Cu 0.6wt.%, Sb 1.1wt.%, Mg 0.9wt.%, Ti 1.3wt.%, B 0.6wt.%, and the balance is Sn and unavoidable impurities.

[0094] The alloy composition of the lead-free solder in Example 5 is: Ag 0.3wt.%, Cu 0.7wt.%, Sb 1.5wt.%, Mg 1.2wt.%, Ti 1.0wt.%, B 0.5wt.%, and the balance is Sn and unavoidable impurities.

[0095] The alloy composition of the lead-free solder in Example 6 is: Ag 0.35wt.%, Cu 0.65wt.%, Sb 0.6wt.%, Mg 0.8wt.%, Ti 2.0wt.%, B 0.3wt.%, and the balance is Sn and inevitable impurities.

[0096] Example 7

[0097] Provided are a low-cost lead-free solder for narrow pitch and high-density packaging technology and a preparation method thereof. The alloy composition of the lead-free solder is: Ag 0.4wt.%, Cu 0.3wt.%, Sb 1.2wt.%, Mg 1.6wt.%, Ti 1.8wt.%, B 0.8wt.%, and the remainder is Sn and unavoidable impurities.

[0098] The preparation method of the lead-free solder comprises the following steps:

[0099] (1) Sn-Cu master alloy, Sn-Ag master alloy, Sn-Sb master alloy, Sn-Ti master alloy and Cu-B master alloy were prepared by induction melting method.

[0100] (2) Using the Sn-Cu master alloy and the Cu-B master alloy in step (1) as raw materials, according to the required alloy ratio, an induction melting method is used to prepare a Sn-Cu-B master alloy. During the melting, the Sn-Cu master alloy is first melted and then the Cu-B master alloy is added and stirred evenly.

[0101] (3) According to the required alloy ratio, the Sn-Ti master alloy and the Sn-Cu-B master alloy are mixed and smelted to obtain the Sn-Cu-Ti-B master alloy.

[0102] (4) Pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy are added into a smelting furnace A according to the required alloy ratio, and mixed and melted to obtain an alloy melt. The smelting temperature is 600° C., and tin chloride is added after the master alloy is completely melted.

[0103] (5) The alloy melt in the melting furnace A is kept at 550° C. for 60 min, and the Sn-Cu-Ti-B master alloy is added and kept warm until it is fully melted to obtain a mixed melt.

[0104] (6) Melting furnace B is preheated at 300°C for 1 h, and metallic Mg is added. Helium is passed through and the temperature is raised to 750°C. The temperature is kept until it is completely melted. Subsequently, the molten magnesium is transferred to the bottom of the mixed melt in melting furnace A through a conveying pipe and kept warm for 20 min. After removing the surface oxide slag, the melt is poured into a mold to obtain a solder alloy ingot.

[0105] Example 8

[0106] Provided is a low-cost lead-free solder for narrow pitch, high-density packaging technology and a preparation method thereof, wherein the preparation method is the same as that of Example 7, except that:

[0107] The alloy composition of the lead-free solder is: Ag 0.15wt.%, Cu 0.4wt.%, Sb 1.8wt.%, Mg 0.3wt.%, Ti 0.6wt.%, B 1.1wt.%, and the balance is Sn and inevitable impurities.

[0108] Example 9

[0109] Provided is a low-cost lead-free solder for narrow pitch, high-density packaging technology and a preparation method thereof, wherein the alloy composition of the lead-free solder is the same as that of Example 3, except that:

[0110] In step (6) of the preparation method, smelting furnace B is first preheated at 250°C for 1.5h, and then metal Mg is added, argon is passed through and the temperature is raised to 700°C, and the temperature is kept until it is completely melted, and then the magnesium melt is transferred to the bottom of smelting furnace A through an infusion tube.

[0111] Example 10

[0112] Provided is a low-cost lead-free solder for narrow pitch, high-density packaging technology and a preparation method thereof, wherein the alloy composition of the lead-free solder is the same as that of Example 6, except that:

[0113] In step (5) of the preparation method, the alloy melt in the smelting furnace A is kept at 520° C. for 50 min, and the Sn-Cu-Ti-B master alloy is added and kept warm until it is fully melted to obtain a mixed melt.

[0114] Comparative Example 1

[0115] Provided are a low-cost lead-free solder for narrow pitch and high-density packaging technology and a preparation method thereof. The alloy composition of the lead-free solder is: 3wt.%, 0.5wt.%, and the remainder is Sn and inevitable impurities.

[0116] The preparation method of the lead-free solder comprises the following steps:

[0117] (1) Sn-Cu master alloy and Sn-Ag master alloy were prepared by induction melting method.

[0118] (2) Pure Sn, Sn-Cu master alloy and Sn-Ag master alloy are added into melting furnace A according to the required ratio. The melting temperature is 550°C. After the master alloy is completely melted, rosin is added and kept warm for 15 minutes. After removing the surface oxide slag, the melt is poured into a mold to obtain a solder alloy ingot.

[0119] Comparative Example 2

[0120] Provided are a low-cost lead-free solder for narrow pitch and high-density packaging technology and a preparation method thereof. The alloy composition of the lead-free solder is: 1wt.%, 0.5wt.%, and the remainder is Sn and inevitable impurities.

[0121] The preparation method of the lead-free solder comprises the following steps:

[0122] (1) Sn-Cu master alloy and Sn-Ag master alloy were prepared by induction melting method.

[0123] (2) Pure Sn, Sn-Cu master alloy and Sn-Ag master alloy are added into melting furnace A according to the required ratio. The melting temperature is 550°C. After the master alloy is completely melted, rosin is added and kept warm for 15 minutes. After removing the surface oxide slag, the melt is poured into a mold to obtain a solder alloy ingot.

[0124] Hereinafter, the lead-free solders prepared in Examples 1-10 of the present invention and Comparative Examples 1-2 are characterized and tested for performance, and their beneficial technical effects are analyzed accordingly.

[0125] 1. Experimental Subjects

[0126] The lead-free solders prepared in Examples 1 to 10 were used as an experimental group.

[0127] The Sn-3.0Ag-0.5Cu solder and Sn-1.0Ag-0.5Cu solder prepared in Comparative Examples 1 and 2 were used as a control group.

[0128] 2. Experimental Methods

[0129] In the present invention, the solders prepared in the embodiments and comparative examples were subjected to relevant performance tests under the same conditions.

[0130] 1. Melting point measurement

[0131] The melting point was measured by STA409PC differential scanning calorimeter (TAInstrument) at a heating rate of 10°C / min. The sample mass was 30 mg. The numerical processing was automatically calculated by the software, and the peak temperature of the DSC curve was recorded as the melting point of the solder.

[0132] 2. Strength and strength attenuation rate test

[0133] 1) Sample preparation

[0134] The tensile specimens and copper welding specimens were prepared according to Japanese Industrial Standard JIS Z3198.

[0135] 2) Shear strength test

[0136] See also Figure 2 As shown, according to the method of GB / T228-2002, the test was performed on an AG-50KNE ​​universal material testing machine with a tensile rate of 2 mm / min. Three samples were tested for each data point and the average value was taken.

[0137] 3) Thermal cycle strength test

[0138] Each solder alloy of each composition was cut into discs with a diameter of 3 mm and a thickness of 0.05 mm. The solder discs were heated to 250°C in castor oil and solidified to form solder balls with a diameter of about 900 μm. The solder balls coated with rosin lightly activated flux were placed on a copper printed circuit board with a 900 μm solder mask opening, and then reflow soldered at a peak temperature of 280°C to form solder joint samples.

[0139] The solder joint samples were placed in a thermal cycle test chamber. The thermal cycle test temperature range was -40℃~125℃, and the endpoint temperature was kept for 10 minutes. The solder joint shear strength was tested after 1000 cycles. The solder joint shear strength test was performed using a solder ball push-pull tester DAGE4000. The pusher height was 90um from the pad, and the pusher speed was 700μm / s. The solder joint strength was measured by the maximum shear force of each sample, and each component solder joint was repeated 8 times to ensure the accuracy of the results.

[0140] 3. Experimental Results

[0141] The experimental results of the experimental group and the control group were statistically analyzed, wherein the solder alloy composition and melting point temperature test results of Examples 1-10 and Comparative Examples 1-2 are shown in Table 1.

[0142] Table 1 Melting temperatures of solder alloys in Examples and Comparative Examples

[0143]

[0144]

[0145] Combining Table 1 and Figure 1 It can be concluded that the lead-free solder obtained by the preparation method of the present invention has uniform structure, fine grains, no segregation of multi-component alloy components and element aggregation, has a lower melting temperature and no low-temperature melting phenomenon below 175°C is found. Although there are individual experimental examples (such as Examples 5-8) with slightly higher melting temperatures, compared with the melting temperatures of the control group, they are within a comparable melting temperature range, have good wettability, and are suitable for the field of soft soldering technology.

[0146] The strength of the lead-free solder in Examples 1-10 after high-temperature aging at 125°C after soldering and after 300 cycles of thermal cycling at -55°C to +125°C were tested, and the results are shown in Table 2.

[0147] Table 2 Statistical table of mechanical properties of solder alloys in the embodiments and comparative examples

[0148]

[0149] It can be seen from Table 2 that the solder alloy of the experimental group of the present invention has good bonding strength after high-temperature constant-temperature aging for 100 hours; it still has high bonding strength after 300 thermal cycles at -55°C to +125°C, indicating that it has good high temperature resistance and temperature cycle resistance reliability.

[0150] The lead-free solder in the embodiment of the present invention can be used as solder for electronic devices in extreme environments.

[0151] In specific applications, the solder joints or welds formed by the solder alloy of the present invention can be fused with the substrate to be soldered by solder paste reflow, wave soldering or hot melting. The above-mentioned lead-free environmentally friendly solder includes preformed solder sheets, solder strips, solder wires, solder balls and solder powders. The above-mentioned substrate to be soldered includes bare Cu, Cu-OSP treatment, tin plating, Ni plating, Ni-Ag plating or Ni-Au plating treatment. Using the solder for welding can obtain electronic circuits and electronic circuit devices with high reliability.

[0152] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A lead-free solder for narrow pitch, high density packaging, characterized in that: The lead-free solder includes the following elements in mass percentage: Ag 0.05wt.%-0.4wt.%, Cu 0.2wt.%-0.8wt.%, Sb 0.1wt.%-2.0wt.%, Mg 0.01wt.%-2.0wt.%, Ti 0.02wt.%-3.5wt.%, B 0.002wt.%-1.5wt.%, and the rest is Sn and inevitable impurities.

2. The lead-free solder according to claim 1, characterized in that The mass percentage of the Ag element is 0.1wt.% to 0.4wt.%; and / or, The mass percentage of the Cu element is 0.3wt.% to 0.8wt.%; and / or, The mass percentage of the Sb element is 0.2wt.% to 1.8wt.%; and / or, The mass percentage of the Mg element is 0.1wt.% to 1.6wt.%; and / or, The mass percentage of the Ti element is 0.05wt.% to 2.5wt.%; and / or, The mass percentage of the B element is 0.1 wt.% to 1.1 wt.%.

3. A method for preparing the lead-free solder according to any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: Sn-Cu, Sn-Ag, Sn-Sb, Sn-Cu-Ti-B master alloys were prepared by induction melting method; Mixing and smelting pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy according to the required ratio to obtain alloy melt; and After the alloy melt is kept at a temperature of 450° C. to 550° C. for a period of time, the Sn-Cu-Ti-B master alloy is added and fully melted to obtain a mixed melt; Magnesium melt is added into the mixed melt, and the mixture is kept warm and poured to obtain a lead-free solder ingot.

4. The preparation method according to claim 3, characterized in that: The preparation of the Sn-Cu-Ti-B master alloy comprises: Sn-Ti master alloy and Cu-B master alloy were prepared by induction melting method. Mixing and smelting the Sn-Cu master alloy and the Cu-B master alloy according to a required ratio to obtain a Sn-Cu-B master alloy; The Sn-Ti master alloy and the Sn-Cu-B master alloy are mixed and smelted according to a required ratio to obtain the Sn-Cu-Ti-B master alloy.

5. The preparation method according to claim 4, characterized in that: The smelting process of the Sn-Cu-B master alloy comprises: melting the Sn-Cu master alloy, adding the Cu-B master alloy, and stirring the mixture evenly.

6. The preparation method according to claim 3, characterized in that: The preparation process of the magnesium melt comprises: Preheat the smelting furnace at 100℃~300℃ for 1h~3h; Add metallic magnesium, raise the temperature to 650℃~750℃ under a protective atmosphere, and keep warm until it is completely melted.

7. The preparation method according to claim 3, characterized in that: The temperature for mixed melting of pure Sn, Sn-Cu master alloy, Sn-Ag master alloy and Sn-Sb master alloy is 500° C. to 600° C.; Preferably, the alloy melt is kept at a temperature of 450° C. to 550° C. for 20 min to 60 min.

8. The preparation method according to claim 3, characterized in that: The magnesium melt is added to the mixed melt and the heat preservation time before pouring is 5 minutes to 30 minutes.

9. The preparation method according to claim 3, characterized in that: The preparation method further comprises converting the lead-free solder ingot into at least one of a paste, a tape, a foil, a sheet, a wire or a powder.

10. Use of the lead-free solder described in any one of claims 1-2 or the lead-free solder prepared by the preparation method described in any one of claims 3-9 as solder for 5G communication electronic devices.