Preparation method of antistatic oriented strand board

The method enhances oriented strand board with durable antistatic and mechanical properties by using graphene oxide and modified zinc oxide treatments, addressing issues of antistatic durability and UV resistance.

CN119077883AActive Publication Date: 2024-12-06寿光市鲁丽木业股份有限公司 +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411227907.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing oriented strand board technologies lack durable antistatic performance, suffer from moisture resistance issues, and experience strength degradation under ultraviolet irradiation.

Method used

A method involving the preparation of antistatic particles through graphene oxide and modified zinc oxide treatments, followed by impregnation, drying, gluing, paving, and hot pressing to create a three-layer structured oriented strand board with enhanced antistatic and mechanical properties.

Benefits of technology

The method results in an oriented strand board with long-lasting antistatic performance, improved mechanical strength, and resistance to ultraviolet degradation, maintaining properties such as density, bending strength, and elastic modulus.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a preparation method of an antistatic oriented strand board, and belongs to the technical field of strand boards. The preparation method comprises the steps of antistatic particle preparation, dipping, drying, sizing, paving, hot press molding and post-treatment. The preparation of the antistatic particles comprises the steps of graphene oxide pretreatment, zinc oxide modification and mixing. The mixing step comprises the following steps: putting pretreated graphene oxide into toluene, uniformly stirring, adding modified zinc oxide, stirring for 33-38 minutes at the stirring speed of 210-230 rpm, raising the temperature to 70-74 DEG C after stirring, adding triethylamine at the adding speed of 2.0-2.4 mL / min, reacting for 6.5-6.8 hours at the temperature of 70-74 DEG C after adding, filtering, washing and drying after the reaction is finished, thereby obtaining the graphene oxide / triethylamine composite material. The antistatic particles are prepared; the antistatic oriented strand board manufactured through the method is good and durable in antistatic performance, high in mechanical property and excellent in ultraviolet resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of particle boards, and in particular relates to a method for preparing an antistatic oriented particle board. Background Art

[0002] Oriented strand board is one of the new varieties of particle board. When the particles are laid out, the upper and lower surface layers of the oriented strand board arrange the glue-mixed particles longitudinally according to their fiber direction, while the core layer particles are arranged transversely to form a three-layer structural slab, which is then hot-pressed into an oriented strand board. The shape of this particle board requires a relatively large length and is slightly thicker than ordinary particle board. There are two methods of directional laying: mechanical orientation and electrostatic orientation. The former is suitable for directional laying of large particles, and the latter is suitable for directional laying of small particles. The directional laying of oriented strand board makes it have higher strength in a certain direction, and it is often used as a structural material instead of plywood.

[0003] Because oriented strand board has a relatively uniform structure and good processing performance, it can be used for decoration and renovation purposes such as indoor furniture, flooring, and indoor doors. It is also the raw material for the construction industry, train and car body manufacturing.

[0004] The prior art for preparing oriented strand boards usually involves increasing the bending elastic modulus, enhancing the static bending strength, etc., and generally does not involve antistatic properties, thereby limiting the use of oriented strand boards.

[0005] For example, CN114800763A discloses a method for preparing a high-strength particleboard, which includes the steps of lignin modification, ultrafine calcium carbonate modification, glue making, glue mixing, particle paving and microwave hot pressing; specifically, it is disclosed that enzymatic lignin is first modified by acrylic acid, itaconic acid and an initiator to obtain modified lignin, and ultrafine calcium carbonate is modified by silane coupling agent and sodium stearate to obtain modified ultrafine calcium carbonate, and then diphenylmethane diisocyanate, polyacrylate, modified lignin and modified ultrafine calcium carbonate are mixed in proportion to obtain composite glue, and then the particles are treated with a pretreatment agent prepared with sodium stearate and sodium chloride, and then the composite glue and particles are mixed to obtain glue-mixed particles, and then the glue-mixed particles are paved to obtain a slab, and then the slab is microwave heated and pressed to obtain a high-strength particleboard.

[0006] The patented particleboard preparation method can heat the oriented particleboard continuously, quickly and evenly, thereby improving the strength performance of the product. However, its antistatic performance is poor, which affects the comprehensive performance of the particleboard.

[0007] In order to improve the antistatic performance of oriented strand board, the applicant added antistatic agent in the early stage of research and development, but there are the following problems: 1. The antistatic agent is easy to lose, making the antistatic performance not lasting; 2. Excessive use of antistatic agents will affect the strength performance of oriented strand board; 3. The moisture resistance of the oriented strand board is poor, and its strength performance drops sharply under ultraviolet irradiation. Summary of the invention

[0008] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing an antistatic oriented strand board, which has excellent and lasting antistatic performance, good strength performance, and excellent UV resistance.

[0009] In view of the above technical problems, the present invention adopts the following technical solutions: A method for preparing an antistatic oriented strand board includes the steps of preparing antistatic particles, impregnation, drying, gluing, paving, hot pressing and post-processing. The specific operations are as follows: 1. Preparation of antistatic particles (1) Graphene oxide pretreatment A. Decentralized processing The graphene oxide is placed in deionized water, polyvinyl pyrrolidone and octadecyl dimethyl benzyl ammonium chloride are added, and ultrasonic treatment is performed, the ultrasonic time is 23-27 minutes, the ultrasonic power is 127-140W, and the ultrasonic frequency is 35-40kHz. After the ultrasonic treatment, the mixture is filtered and washed, and dried at 78-82°C for 8.8-9.2 hours to obtain dispersed graphene oxide; The mass ratio of the graphene oxide, deionized water, polyvinyl pyrrolidone and octadecyl dimethyl benzyl ammonium chloride is 7.2-7.6:60-65:0.7-0.9:0.8-1.2; B. Secondary Processing The dispersed graphene oxide and tetrahydrofuran are placed in a reaction container and stirred for 30-34 minutes at a stirring speed of 242-257 rpm. After the stirring is completed, nitrogen is introduced, hexachlorocyclotriphosphazene and triethylamine are added, and the temperature is raised from 0.8-1.2° C. to 73-77° C. for reflux reaction for 12.0-13.0 hours. After the reaction is completed, the mixture is filtered, washed and dried to obtain pretreated graphene oxide; The mass volume ratio of the dispersed graphene oxide, tetrahydrofuran, hexachlorocyclotriphosphazene and triethylamine is 5.4-5.8 g:95-110 mL:11.8-12.2 g:19.7-20.3 g; (2) Preparation of modified zinc oxide A. Primary modification The zinc oxide is placed in an ethanol solution and subjected to ball milling treatment. The ball milling time is 30-34 minutes, the ball milling speed is 104-116 rpm, the ball milling temperature is 43-47° C., and the ball-to-material ratio is 4-6:1. After the ball milling is completed, the zinc oxide is transferred to a closed container, an amination reagent is added, and after stirring evenly, the temperature is increased to 70-73° C., the pressure is controlled to be 1.4-1.6 MPa, and the zinc oxide is allowed to stand for 6.3-6.7 hours. After the standing period is completed, the zinc oxide is filtered, washed, and dried to obtain primary modified zinc oxide. The particle size of the zinc oxide is 175-185 nm; The mass concentration of the ethanol solution is 50-54%; The mass ratio of the zinc oxide, the ethanol solution and the amination reagent is 10.1-10.5:115-125:2.7-3.0; The aminating agent is a mixture of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate, and the mass ratio of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate is 0.8-1.2:0.6-0.8:1.1-1.4; B. Deep modification Add ethanol solution and tartaric acid to the reaction container, stir evenly, add primary modified zinc oxide, control the addition rate to be 0.4-0.6 g / min, perform ultrasonic treatment after the addition is completed, the ultrasonic time is 13-17 min, the ultrasonic power is 94-98 W, the ultrasonic frequency is 30-35 kHz, after the ultrasonic treatment is completed, heat to 80-84° C. at a rate of 0.4-0.6° C. / min, stir to react for 18-22 h, filter and dry after the stirring reaction is completed, and obtain modified zinc oxide; The mass concentration of the ethanol solution is 38-43%; The mass volume ratio of the ethanol solution, tartaric acid, and primary modified zinc oxide is 95-105 mL: 5.0-5.3 g: 3.5-3.8 g; (3) Mixed The pretreated graphene oxide is placed in toluene, and after stirring evenly, the modified zinc oxide is added and stirred for 33-38 minutes, and the stirring speed is 210-230 rpm. After the stirring is completed, the temperature is increased to 70-74°C, and triethylamine is added, and the addition rate is controlled to be 2.0-2.4 mL / min. After the addition is completed, the reaction is carried out at 70-74°C for 6.5-6.8 hours. After the reaction is completed, the antistatic particles are obtained by filtering, washing, and drying. The mass ratio of the pretreated graphene oxide, toluene, modified zinc oxide and triethylamine is 1.8-2.2 g: 37-42 mL: 3.6-3.8 g: 21-25 mL.

[0010] 2. Impregnation The surface shavings and the core shavings are placed in an antistatic composite agent respectively, stirred evenly and then immersed for 13-18 minutes at a temperature of 36-40° C. After the immersion, the immersed surface shavings and the immersed core shavings are obtained respectively; The surface shavings are 35-38 mm long, 4.3-4.7 mm wide and 0.20-0.25 mm thick, and are made from poplar shavings; The core material is 40-44 mm long, 4.8-5.2 mm wide, and 0.22-0.28 mm thick, and is made of pine wood chips; The mass ratio of the surface wood chips raw material to the antistatic composite agent is 5.3-5.6:18-20; The mass ratio of the core layer wood chips raw material to the antistatic agent is 4.1-4.3:21-25; The raw material components of the antistatic composite are 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide, and the mass ratio of the 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide is 86-90:18-22:3.7-4.3:3.0-3.4:8.3-8.7.

[0011] 3. Drying The impregnated surface wood chips and the impregnated core wood chips are dried using flue gas at 348-354° C. respectively, so that the moisture content is 2.3-2.7%, thereby obtaining dried surface wood chips and dried core wood chips.

[0012] 4. Gluing Adhesive is applied to the dried surface wood chips and the dried core wood chips by mechanically mixing adhesive to obtain the glued surface wood chips and the glued core wood chips; The amount of glue applied on the surface layer is 2.5-3.0%, and the amount of glue applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The amount of glue applied to the core layer is 2.1-2.5%, and the amount applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The preparation method of the adhesive comprises the following steps: mixing 32-37 g of isocyanate glue and 4.0-4.4 g of nano titanium dioxide, stirring evenly, adding 1.8-2.2 g of paraffin, 1.2-1.4 g of diacetyl tartaric acid monoglyceride and 1.6-1.8 g of sodium oleate for homogenization, wherein the homogenization time is 4.5-5.5 min and the homogenization pressure is 4.4-4.8 MPa. After the homogenization is completed, the adhesive is obtained.

[0013] 5. Paving The glued core layer wood chips are paved through a five-layer paving head to obtain a core layer material, and then the glued surface layer material is paved on the upper and lower surfaces of the core layer material to obtain a slab; The core layer material is a three-layer structure, which is composed of a core layer upper surface layer, a core layer middle layer, and a core layer lower surface layer from top to bottom, wherein the core layer middle layer is paved horizontally, and the core layer upper surface layer and the core layer lower surface layer are paved vertically; When the surface material is paved, the surface wood chips after gluing are arranged longitudinally; The mass ratio of the core layer material to the surface layer material is 7.3-7.7:2.3-2.7; In the core layer material, the mass ratio of the core layer upper surface layer, the core layer middle layer, and the core layer lower surface layer is 1:0.8-1.2:1; The mass ratio of the upper layer to the lower layer of the surface material is 1:0.8-1.2.

[0014] 6. Heat pressing The slab is compacted by a pre-pressing machine, and then cut into the required slab width by a slab trimming saw to obtain a sawn slab, and the slab is hot pressed by a continuous flat press. The hot pressing temperatures are 232-237°C, 218-224°C, 216-222°C, 198-202°C, and 167-173°C, respectively. The hot pressing factor is 5.8-6.2s / mm, and the pressures are 1.3-1.5MPa, 1.2-1.4MPa, 0.8-1.0MPa, 0.4-0.6MPa, and 0.7-0.9MPa, respectively. After the hot pressing is completed, a plain board is obtained.

[0015] 7. Post-processing Oriented strand board is produced by cross-cutting, turning over for cooling, aging and storage, cutting to specifications, inspecting and grading, and packaging for storage.

[0016] Compared with the prior art, the present invention has achieved the following beneficial effects: 1. The present invention firstly performs a dispersion treatment on graphene oxide, which can better avoid the agglomeration of graphene and enhance the dispersion performance. Then, hexachlorocyclotriphosphazene is used for secondary treatment. Under the catalytic action of triethylamine, the hydroxyl group of graphene oxide can react with hexachlorocyclotriphosphazene, and hexachlorocyclotriphosphazene is grafted on the surface of graphene oxide. The obtained pretreated graphene oxide has good stability. In the step of preparing modified zinc oxide, aminosilane coupling agent is firstly used to perform primary modification on zinc oxide, so that the primary modified oxide Zinc is present as particles dispersed separately and grafted with amino groups on the surface, and then tartaric acid is used for condensation acylation reaction, and finally after a mixing step, the P-Cl group of the pretreated graphene oxide reacts with the -NH2 of the modified zinc oxide to obtain antistatic particles, and the zinc oxide and graphene oxide present a cross-linked network structure with strong and stable binding force. The particles are used in the impregnation and sizing steps, have good compatibility with other components, good homogeneity, and effectively enhance the antistatic properties and mechanical properties of the oriented strand board, and the antistatic properties are long-lasting and the mechanical properties are stable; 2. The antistatic oriented strand board prepared by the method of the present invention has a density of 0.84-0.89 g / cm 3 ; 3. The antistatic oriented strand board prepared by the method of the present invention has a parallel static bending strength of 46.7-47.4 MPa, a vertical static bending strength of 30.6-31.2 MPa, an internal bonding strength of 0.84-0.92 MPa, and a parallel elastic modulus of 4885-4894 MPa; 4. The antistatic oriented strand board prepared by the method of the present invention has good and durable antistatic performance and a resistivity of 3.25-3.32×10 7 Ω / cm; 5. The antistatic oriented strand board prepared by the method of the present invention is placed at a strength of 610W / cm 2 The samples were irradiated with ultraviolet light for 5 days and then placed at an intensity of 820 W / cm 2 The samples were irradiated with ultraviolet light for 5 days and then placed in a vacuum tube with an intensity of 450 W / cm 2 After irradiation under ultraviolet light for 5 days, the parallel static bending strength was measured again to be 44.0-45.2MPa, the vertical static bending strength was 28.5-29.4MPa, and the parallel elastic modulus was 4631-4703MPa. DETAILED DESCRIPTION

[0017] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.

[0018] Example 1 1. Preparation of antistatic particles (1) Graphene oxide pretreatment A. Decentralized processing 7.4 g of graphene oxide was placed in 63 g of deionized water, 0.8 g of polyvinyl pyrrolidone and 1.0 g of octadecyl dimethyl benzyl ammonium chloride were added, and ultrasonic treatment was performed. The ultrasonic time was 25 min, the ultrasonic power was 132 W, and the ultrasonic frequency was 37 kHz. After the ultrasonic treatment, the mixture was filtered and washed, and dried at 80 ° C for 9.0 h to obtain dispersed graphene oxide. B. Secondary Processing 5.6 g of dispersed graphene oxide and 100 mL of tetrahydrofuran were placed in a reaction container and stirred for 32 min at a stirring speed of 250 rpm. After the stirring was completed, nitrogen was introduced, 12.0 g of hexachlorocyclotriphosphazene and 20.0 g of triethylamine were added, the temperature was raised from 1.0° C. to 75° C., and a reflux reaction was performed for 12.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain pretreated graphene oxide; (2) Preparation of modified zinc oxide A. Primary modification 10.3 g of zinc oxide was placed in 120 g of ethanol solution and ball-milled. The ball-milling time was 32 min, the ball-milling speed was 110 rpm, the ball-milling temperature was 45 ° C, and the ball-to-material ratio was 5:1. After the ball-milling was completed, it was transferred to a closed container, 2.9 g of amination reagent was added, and after stirring evenly, the temperature was increased to 71 ° C, the pressure was controlled to 1.5 MPa, and it was allowed to stand for 6.5 h. After the standing period, it was filtered, washed, and dried to obtain primary modified zinc oxide; The particle size of the zinc oxide is 180 nm; The mass concentration of the ethanol solution is 52%; The aminating agent is a mixture of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate, and the mass ratio of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate is 1.0:0.7:1.2; B. Deep modification Add 100 mL of ethanol solution and 5.1 g of tartaric acid to the reaction container, stir evenly, then add 3.7 g of primary modified zinc oxide, control the addition rate to be 0.5 g / min, perform ultrasonic treatment after the addition is completed, the ultrasonic time is 15 min, the ultrasonic power is 96 W, the ultrasonic frequency is 33 kHz, after the ultrasonic treatment is completed, heat to 82 ° C at a rate of 0.5 ° C / min, stir and react for 20 h, after the stirring reaction is completed, filter and dry to obtain modified zinc oxide; The mass concentration of the ethanol solution is 40%; (3) Mixed 2.0 g of pretreated graphene oxide was placed in 40 mL of toluene, and after stirring evenly, 3.7 g of modified zinc oxide was added and stirred for 35 min at a stirring speed of 220 rpm. After stirring, the temperature was raised to 72 °C, 23 mL of triethylamine was added, and the addition rate was controlled at 2.2 mL / min. After the addition was completed, the reaction was carried out at 72 °C for 6.7 h. After the reaction was completed, the antistatic particles were obtained by filtration, washing and drying.

[0019] 2. Impregnation The surface shavings and the core shavings are placed in the antistatic composite agent respectively, stirred evenly and then immersed, the immersion time is 15 minutes, the immersion temperature is 38°C, and after the immersion, the immersed surface shavings and the immersed core shavings are obtained respectively; The surface shavings are 36 mm long, 4.5 mm wide and 0.23 mm thick and are made from poplar shavings; The core material is 42 mm long, 5.0 mm wide and 0.25 mm thick and is made of pine wood chips; The mass ratio of the surface wood chips raw material to the antistatic composite agent is 5.4:19; The mass ratio of the core layer wood chips to the antistatic agent is 4.2:23; The raw material components of the antistatic composite are 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide, and the mass ratio of the 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide is 88:20:4.0:3.2:8.5.

[0020] 3. Drying The impregnated surface wood chips and the impregnated core wood chips were dried using 350° C. flue gas to make the moisture content 2.5%, thereby obtaining dried surface wood chips and dried core wood chips.

[0021] 4. Gluing Adhesive is applied to the dried surface wood chips and the dried core wood chips by mechanically mixing adhesive to obtain the glued surface wood chips and the glued core wood chips; The amount of glue applied on the surface layer is 2.7%, and the amount of glue applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The amount of glue applied to the core layer is 2.3%, and the amount applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The preparation method of the adhesive is as follows: 35g of isocyanate glue and 4.2g of nano titanium dioxide are mixed, stirred evenly, and then 2.0g of paraffin, 1.3g of diacetyl tartaric acid monoglyceride and 1.7g of sodium oleate are added for homogenization treatment, the homogenization time is 5.0min, the homogenization pressure is 4.6MPa, and after the homogenization treatment is completed, the adhesive is obtained.

[0022] 5. Paving The glued core layer wood chips are paved through a five-layer paving head to obtain a core layer material, and then the glued surface layer material is paved on the upper and lower surfaces of the core layer material to obtain a slab; The core layer material is a three-layer structure, which is composed of a core layer upper surface layer, a core layer middle layer, and a core layer lower surface layer from top to bottom, wherein the core layer middle layer is paved horizontally, and the core layer upper surface layer and the core layer lower surface layer are paved vertically; When the surface material is paved, the surface wood chips after gluing are arranged longitudinally; The mass ratio of the core layer material to the surface layer material is 7.5:2.5; In the core layer material, the mass ratio of the core layer upper surface layer, the core layer middle layer, and the core layer lower surface layer is 1:1:1; The mass ratio of the upper layer to the lower layer of the surface material is 1:1.

[0023] 6. Heat pressing The slab is compacted by a pre-pressing machine, and then cut into the required slab width by a slab trimming saw to obtain a sawn slab. The slab is hot pressed by a continuous flat press. The hot pressing temperatures are 235°C, 220°C, 220°C, 200°C, and 170°C, respectively. The hot pressing factor is 6s / mm, and the pressures are 1.4MPa, 1.3MPa, 0.9MPa, 0.5MPa, and 0.8MPa, respectively. After the hot pressing, a plain board is obtained.

[0024] 7. Post-processing Oriented strand board is produced by cross-cutting, turning over for cooling, aging and storage, cutting to specifications, inspecting and grading, and packaging for storage.

[0025] Example 2 1. Preparation of antistatic particles (1) Graphene oxide pretreatment A. Decentralized processing 7.2 g of graphene oxide was placed in 60 g of deionized water, 0.7 g of polyvinyl pyrrolidone and 0.8 g of octadecyl dimethyl benzyl ammonium chloride were added, and ultrasonic treatment was performed. The ultrasonic time was 23 min, the ultrasonic power was 127 W, and the ultrasonic frequency was 35 kHz. After the ultrasonic treatment, the mixture was filtered and washed, and dried at 78 ° C for 8.8 h to obtain dispersed graphene oxide. B. Secondary Processing 5.4 g of dispersed graphene oxide and 95 mL of tetrahydrofuran were placed in a reaction container and stirred for 30 min at a stirring speed of 242 rpm. After the stirring was completed, nitrogen was introduced, 11.8 g of hexachlorocyclotriphosphazene and 19.7 g of triethylamine were added, the temperature was raised from 0.8° C. to 73° C., and a reflux reaction was performed for 12.0 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain pretreated graphene oxide; (2) Preparation of modified zinc oxide A. Primary modification 10.1g zinc oxide was placed in 115g ethanol solution and ball milled. The ball milling time was 30min, the ball milling speed was 104rpm, the ball milling temperature was 43°C, and the ball-to-material ratio was 4:1. After the ball milling was completed, it was transferred to a closed container, 2.7g amination reagent was added, and after stirring evenly, the temperature was increased to 70°C, the pressure was controlled to 1.4MPa, and it was allowed to stand for 6.3h. After the standing period was completed, it was filtered, washed, and dried to obtain primary modified zinc oxide; The particle size of the zinc oxide is 175 nm; The mass concentration of the ethanol solution is 50%; The aminating agent is a mixture of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate, and the mass ratio of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate is 0.8:0.6:1.1; B. Deep modification Add 95 mL of ethanol solution and 5.0 g of tartaric acid to the reaction container, stir evenly, then add 3.5 g of primary modified zinc oxide, control the addition rate to be 0.4 g / min, perform ultrasonic treatment after the addition is completed, the ultrasonic time is 13 min, the ultrasonic power is 94 W, the ultrasonic frequency is 30 kHz, after the ultrasonic treatment is completed, heat to 80 ° C at a rate of 0.4 ° C / min, stir and react for 18 h, after the stirring reaction is completed, filter and dry to obtain modified zinc oxide; The mass concentration of the ethanol solution is 38%; (3) Mixed 1.8 g of pretreated graphene oxide was placed in 37 mL of toluene, and after stirring evenly, 3.6 g of modified zinc oxide was added and stirred for 33 min at a stirring speed of 210 rpm. After stirring, the temperature was raised to 70 ° C, 21 mL of triethylamine was added, and the addition rate was controlled to be 2.0 mL / min. After the addition was completed, the reaction was carried out at 70 ° C for 6.5 h. After the reaction was completed, the antistatic particles were obtained by filtration, washing and drying.

[0026] 2. Impregnation The surface shavings and the core shavings are placed in the antistatic composite agent respectively, stirred evenly and then immersed, the immersion time is 13 minutes, the immersion temperature is 36°C, and after the immersion, the immersed surface shavings and the immersed core shavings are obtained respectively; The surface shavings are 35 mm long, 4.3 mm wide and 0.20 mm thick and are made from poplar shavings. The core material is 40 mm long, 4.8 mm wide and 0.22 mm thick and is made of pine wood chips; The mass ratio of the surface wood chips raw material to the antistatic composite agent is 5.3:18; The mass ratio of the core layer wood chips to the antistatic agent is 4.1:21; The raw material components of the antistatic composite are 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide, and the mass ratio of the 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide is 86:18:3.7:3.0:8.3.

[0027] 3. Drying The impregnated surface wood chips and the impregnated core wood chips were dried using flue gas at 348° C. to make the moisture content 2.3%, thereby obtaining dried surface wood chips and dried core wood chips.

[0028] 4. Gluing Adhesive is applied to the dried surface wood chips and the dried core wood chips by mechanically mixing adhesive to obtain the glued surface wood chips and the glued core wood chips; The amount of glue applied on the surface layer is 2.5%, and the amount of glue applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The amount of glue applied to the core layer is 2.1%, and the amount applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The preparation method of the adhesive is as follows: 32g of isocyanate glue and 4.0g of nano titanium dioxide are mixed, stirred evenly, and then 1.8g of paraffin, 1.2g of diacetyl tartaric acid monoglyceride and 1.6g of sodium oleate are added for homogenization treatment, the homogenization time is 4.5min, the homogenization pressure is 4.8MPa, and after the homogenization treatment is completed, the adhesive is obtained.

[0029] 5. Paving The glued core layer wood chips are paved through a five-layer paving head to obtain a core layer material, and then the glued surface layer material is paved on the upper and lower surfaces of the core layer material to obtain a slab; The core layer material is a three-layer structure, which is composed of a core layer upper surface layer, a core layer middle layer, and a core layer lower surface layer from top to bottom, wherein the core layer middle layer is paved horizontally, and the core layer upper surface layer and the core layer lower surface layer are paved vertically; When the surface material is paved, the surface wood chips after gluing are arranged longitudinally; The mass ratio of the core layer material to the surface layer material is 7.3:2.7; In the core layer material, the mass ratio of the core layer upper surface layer, the core layer middle layer, and the core layer lower surface layer is 1:1.2:1; The mass ratio of the upper layer to the lower layer of the surface material is 1:0.8.

[0030] 6. Heat pressing The slab is compacted by a pre-pressing machine, and then cut into the required slab width by a slab trimming saw to obtain a sawn slab. The slab is hot pressed by a continuous flat press. The hot pressing temperatures are 232°C, 218°C, 216°C, 198°C, and 167°C, respectively. The hot pressing factor is 5.8s / mm, and the pressures are 1.3MPa, 1.2MPa, 0.8MPa, 0.4MPa, and 0.7MPa, respectively. After the hot pressing, a plain board is obtained.

[0031] 7. Post-processing Oriented strand board is produced by cross-cutting, turning over for cooling, aging and storage, cutting to specifications, inspecting and grading, and packaging for storage.

[0032] Example 3 1. Preparation of antistatic particles (1) Graphene oxide pretreatment A. Decentralized processing 7.6 g of graphene oxide was placed in 65 g of deionized water, 0.97 g of polyvinyl pyrrolidone and 1.2 g of octadecyl dimethyl benzyl ammonium chloride were added, and ultrasonic treatment was performed. The ultrasonic time was 27 min, the ultrasonic power was 140 W, and the ultrasonic frequency was 40 kHz. After the ultrasonic treatment, the mixture was filtered and washed, and dried at 82 ° C for 9.2 h to obtain dispersed graphene oxide. B. Secondary Processing 5.8 g of dispersed graphene oxide and 110 mL of tetrahydrofuran were placed in a reaction container and stirred for 34 min at a stirring speed of 257 rpm. After the stirring was completed, nitrogen was introduced, 12.2 g of hexachlorocyclotriphosphazene and 20.3 g of triethylamine were added, the temperature was raised from 1.2° C. to 77° C., and a reflux reaction was performed for 13.0 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain pretreated graphene oxide. (2) Preparation of modified zinc oxide A. Primary modification 10.5 g of zinc oxide was placed in 125 g of ethanol solution and ball-milled. The ball-milling time was 34 min, the ball-milling speed was 116 rpm, the ball-milling temperature was 47 ° C, and the ball-to-material ratio was 6:1. After the ball-milling was completed, it was transferred to a closed container, 3.0 g of amination reagent was added, and after stirring evenly, the temperature was increased to 73 ° C, the pressure was controlled to 1.6 MPa, and it was allowed to stand for 6.7 h. After the standing period, it was filtered, washed, and dried to obtain primary modified zinc oxide; The particle size of the zinc oxide is 185 nm; The mass concentration of the ethanol solution is 54%; The aminating agent is a mixture of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate, and the mass ratio of 3-diethylenetriaminopropyl trimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate is 1.2:0.8:1.4; B. Deep modification Add 105 mL of ethanol solution and 5.3 g of tartaric acid to the reaction container, stir evenly, then add 3.8 g of primary modified zinc oxide, control the addition rate to be 0.6 g / min, perform ultrasonic treatment after the addition is completed, the ultrasonic time is 17 min, the ultrasonic power is 98 W, the ultrasonic frequency is 35 kHz, after the ultrasonic treatment is completed, heat to 84 ° C at a rate of 0.6 ° C / min, stir and react for 22 h, after the stirring reaction is completed, filter and dry to obtain modified zinc oxide; The mass concentration of the ethanol solution is 43%; (3) Mixed 2.2 g of pretreated graphene oxide was placed in 42 mL of toluene, and after stirring evenly, 3.8 g of modified zinc oxide was added and stirred for 38 min at a stirring speed of 230 rpm. After stirring, the temperature was raised to 74 °C, 25 mL of triethylamine was added, and the addition rate was controlled to be 2.4 mL / min. After the addition was completed, the reaction was carried out at 74 °C for 6.8 h. After the reaction was completed, the antistatic particles were obtained by filtration, washing and drying.

[0033] 2. Impregnation The surface shavings and the core shavings are placed in an antistatic composite agent respectively, stirred evenly and then immersed, the immersion time is 18 minutes, the immersion temperature is 40°C, and after the immersion is completed, the immersed surface shavings and the immersed core shavings are obtained respectively; The surface shavings are 38 mm long, 4.7 mm wide and 0.25 mm thick and are made from poplar shavings. The core material is 44 mm long, 5.2 mm wide and 0.28 mm thick and is made of pine wood chips; The mass ratio of the surface wood chips raw material to the antistatic composite agent is 5.6:20; The mass ratio of the core layer wood chips to the antistatic agent is 4.3:25; The raw material components of the antistatic composite are 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide, and the mass ratio of the 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide is 90:22:4.3:3.4:8.7.

[0034] 3. Drying The impregnated surface wood chips and the impregnated core wood chips were dried using flue gas at 354° C. to make the moisture content 2.7%, thereby obtaining dried surface wood chips and dried core wood chips.

[0035] 4. Gluing Adhesive is applied to the dried surface wood chips and the dried core wood chips by mechanically mixing adhesive to obtain the glued surface wood chips and the glued core wood chips; The surface glue application amount is 3.0%, and the glue application amount is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The amount of glue applied to the core layer is 2.5%, and the amount applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The preparation method of the adhesive is as follows: 37g of isocyanate glue and 4.4g of nano titanium dioxide are mixed, stirred evenly, and then 2.2g of paraffin, 1.4g of diacetyl tartaric acid monoglyceride and 1.8g of sodium oleate are added for homogenization treatment, the homogenization time is 5.5min, the homogenization pressure is 4.4MPa, and after the homogenization treatment is completed, the adhesive is obtained.

[0036] 5. Paving The glued core layer wood chips are paved through a five-layer paving head to obtain a core layer material, and then the glued surface layer material is paved on the upper and lower surfaces of the core layer material to obtain a slab; The core layer material is a three-layer structure, which is composed of a core layer upper surface layer, a core layer middle layer, and a core layer lower surface layer from top to bottom, wherein the core layer middle layer is paved horizontally, and the core layer upper surface layer and the core layer lower surface layer are paved vertically; When the surface material is paved, the surface wood chips after gluing are arranged longitudinally; The mass ratio of the core layer material to the surface layer material is 7.7:2.3; In the core layer material, the mass ratio of the core layer upper surface layer, the core layer middle layer, and the core layer lower surface layer is 1:0.8:1; The mass ratio of the upper layer to the lower layer of the surface material is 1:1.2.

[0037] 6. Heat pressing The slab is compacted by a pre-pressing machine, and then cut into the required slab width by a slab trimming saw to obtain a sawn slab. The slab is hot pressed by a continuous flat press. The hot pressing temperatures are 237°C, 224°C, 222°C, 202°C, and 173°C, respectively. The hot pressing factor is 6.2s / mm, and the pressures are 1.5MPa, 1.4MPa, 1.0MPa, 0.6MPa, and 0.9MPa, respectively. After the hot pressing, a plain board is obtained.

[0038] 7. Post-processing Oriented strand board is produced by cross-cutting, turning over for cooling, aging and storage, cutting to specifications, inspecting and grading, and packaging for storage.

[0039] Comparative Example 1 Based on Example 1, the change is that in the step of preparing the antistatic particles, (1) Omitting the secondary treatment step of the graphene oxide pretreatment step; (2) In the step of preparing modified zinc oxide, the deep modification step is omitted; (3) in the mixing step, the pretreated graphene oxide is replaced by dispersed graphene oxide in equal amounts, and the modified zinc oxide is replaced by primary modified zinc oxide in equal amounts; The rest of the operations are the same.

[0040] Comparative Example 2 Based on Example 1, the change is that in the step of preparing the antistatic particles, (1) Omitting the dispersion treatment step of the graphene oxide pretreatment step; (2) In the primary modification step of preparing modified zinc oxide, octylphenol polyoxyethylene ether and glyceryl monostearate in the amination reagent are replaced with 52 wt % ethanol solution in equal amounts; (3) In the gluing step, diacetyl tartaric acid monoglyceride and sodium oleate in the adhesive are replaced with isocyanate glue in equal amounts; The rest of the operations are the same.

[0041] Performance Testing The properties of the oriented strand boards prepared in Examples 1-3 and Comparative Examples 1-2 were tested as follows: 1. Strength performance

[0042] 2. Antistatic properties

[0043] 3. UV resistance The oriented strand boards prepared in Examples 1-3 and Comparative Examples 1-2 were placed on a plate with a strength of 610 W / cm 2The samples were irradiated with ultraviolet light for 5 days and then placed at an intensity of 820 W / cm 2 The samples were irradiated with ultraviolet light for 5 days and then placed in a vacuum tube with an intensity of 450 W / cm 2 After irradiation under ultraviolet light for 5 days, the strength performance was tested again. The results are as follows:

[0044] Both graphene oxide and zinc oxide have good antistatic properties, but they have poor dispersibility and poor compatibility with components such as isocyanate glue, which affects the comprehensive performance of particleboard. In the present invention, the graphene oxide is first dispersed to better avoid the agglomeration of graphene and enhance the dispersion performance. Then, hexachlorocyclotriphosphazene is used for secondary treatment. Under the catalytic action of triethylamine, the hydroxyl group of the graphene oxide can react with hexachlorocyclotriphosphazene, and hexachlorocyclotriphosphazene is grafted on the surface of the graphene oxide. The obtained pretreated graphene oxide has good stability. In the step of preparing the modified zinc oxide, first Zinc oxide is primarily modified by using an aminosilane coupling agent, so that the primary modified zinc oxide presents particles that are individually dispersed and have amino groups grafted on the surface, and then tartaric acid is used for condensation acylation reaction, and finally after a mixing step, the P-Cl group of the pretreated graphene oxide reacts with -NH2 of the modified zinc oxide to obtain antistatic particles, and the zinc oxide and graphene oxide present a cross-linked network structure with strong and stable bonding force. The antistatic particles are used in the impregnation and sizing steps, have good compatibility with other components, and good homogeneity, and effectively enhance the antistatic properties and mechanical properties of the oriented strand board, and the antistatic properties are long-lasting and the mechanical properties are stable.

[0045] In comparative example 1, in the mixing step, the pretreated graphene oxide is replaced by dispersed graphene oxide in equal amounts, and the modified zinc oxide is replaced by primary modified zinc oxide in equal amounts. The bonding force between graphene oxide and primary modified zinc oxide is poor, and a relatively stable network structure cannot be formed, which affects the antistatic and mechanical properties of the particleboard, and the ultraviolet radiation resistance is poor; in comparative example 2, the dispersion treatment step of the graphene pretreatment step is omitted. When hexachlorocyclotriphosphazene is used for secondary treatment, the grafting of graphene oxide is insufficient. In the primary modification step of the modified zinc oxide, the modification of the aminosilane coupling agent is also insufficient, which makes its reaction in the mixing step uneven, affecting the structural uniformity of the antistatic particles. In addition, in the sizing step, the diacetyl tartaric acid monoglyceride and sodium oleate in the adhesive are replaced by isocyanate glue in equal amounts, which leads to the dispersibility and wetting properties of the adhesive, and ultimately leads to poor mechanical properties and poor stability of the oriented strand board.

[0046] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.

[0047] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an antistatic oriented strand board, characterized in that: The preparation method comprises the steps of preparing antistatic particles, impregnation, drying, sizing, paving, hot pressing and post-processing; The preparation of antistatic particles comprises graphene oxide pretreatment, zinc oxide modification and mixing steps; The graphene oxide pretreatment step includes a dispersion treatment and a secondary treatment step; The dispersion treatment step comprises placing graphene oxide in deionized water, adding polyvinyl pyrrolidone and octadecyl dimethyl benzyl ammonium chloride, and performing ultrasonic treatment, wherein the ultrasonic time is 23-27 minutes, the ultrasonic power is 127-140W, and the ultrasonic frequency is 35-40kHz. After the ultrasonic treatment, filtering and washing are performed, and drying is performed at 78-82°C for 8.8-9.2 hours to obtain dispersed graphene oxide; The secondary treatment step comprises placing dispersed graphene oxide and tetrahydrofuran in a reaction container, stirring for 30-34 minutes, and stirring at a speed of 242-257 rpm. After the stirring is completed, nitrogen is introduced, hexachlorocyclotriphosphazene and triethylamine are added, and the temperature is raised from 0.8-1.2° C. to 73-77° C. for reflux reaction for 12.0-13.0 hours. After the reaction is completed, the pretreated graphene oxide is obtained by filtering, washing, and drying. The modified zinc oxide comprises primary modification and deep modification steps; The zinc oxide is placed in an ethanol solution and subjected to ball milling treatment. The ball milling time is 30-34 minutes, the ball milling speed is 104-116 rpm, the ball milling temperature is 43-47° C., and the ball-to-material ratio is 4-6:

1. After the ball milling is completed, the zinc oxide is transferred to a closed container, an amination reagent is added, and after stirring evenly, the temperature is increased to 70-73° C., the pressure is controlled to be 1.4-1.6 MPa, and the zinc oxide is allowed to stand for 6.3-6.7 hours. After the standing period is completed, the zinc oxide is filtered, washed, and dried to obtain primary modified zinc oxide. The aminating agent is a mixture of 3-diethylenetriaminopropyltrimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate; The deep modification step comprises: adding ethanol solution and tartaric acid to a reaction container, stirring evenly, adding primary modified zinc oxide, controlling the adding rate to be 0.4-0.6 g / min, performing ultrasonic treatment after the addition is completed, the ultrasonic time is 13-17 min, the ultrasonic power is 94-98 W, the ultrasonic frequency is 30-35 kHz, after the ultrasonic treatment is completed, heating to 80-84° C. at a rate of 0.4-0.6° C. / min, stirring for reaction for 18-22 h, filtering and drying after the stirring reaction is completed, and obtaining modified zinc oxide; The mixing step comprises placing the pretreated graphene oxide in toluene, stirring evenly, adding modified zinc oxide and stirring for 33-38 minutes, and stirring at a speed of 210-230 rpm. After stirring, the temperature is raised to 70-74° C., and triethylamine is added at a rate of 2.0-2.4 mL / min. After the addition is completed, the reaction is carried out at 70-74° C. for 6.5-6.8 hours. After the reaction is completed, the antistatic particles are obtained by filtering, washing, and drying.

2. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: In the graphene oxide pretreatment step, in the dispersion treatment step, the mass ratio of the graphene oxide, deionized water, polyvinyl pyrrolidone and octadecyl dimethyl benzyl ammonium chloride is 7.2-7.6:60-65:0.7-0.9:0.8-1.2; In the secondary treatment step, the mass volume ratio of the dispersed graphene oxide, tetrahydrofuran, hexachlorocyclotriphosphazene and triethylamine is 5.4-5.8 g:95-110 mL:11.8-12.2 g:19.7-20.3 g.

3. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: In the primary modification step, the particle size of the zinc oxide is 175-185 nm; The mass concentration of the ethanol solution is 50-54%; The mass ratio of the zinc oxide, the ethanol solution and the amination reagent is 10.1-10.5:115-125:2.7-3.0; The mass ratio of the 3-diethylenetriaminopropyltrimethoxysilane, octylphenol polyoxyethylene ether and glyceryl monostearate is 0.8-1.2:0.6-0.8:1.1-1.

4.

4. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: In the deep modification step, the mass concentration of the ethanol solution is 38-43%; The mass volume ratio of the ethanol solution, tartaric acid and primary modified zinc oxide is 95-105 mL: 5.0-5.3 g: 3.5-3.8 g.

5. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: In the mixing step, the mass ratio of the pretreated graphene oxide, toluene, modified zinc oxide, and triethylamine is 1.8-2.2 g: 37-42 mL: 3.6-3.8 g: 21-25 mL.

6. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: The impregnation step comprises placing the surface shavings and the core shavings in an antistatic composite agent respectively, stirring them evenly and then impregnating them. The impregnation time is 13-18 minutes and the impregnation temperature is 36-40° C. After the impregnation is completed, the impregnated surface shavings and the impregnated core shavings are respectively obtained. The mass ratio of the surface wood chips raw material to the antistatic composite agent is 5.3-5.6:18-20; The mass ratio of the core layer wood chips raw material to the antistatic agent is 4.1-4.3:21-25; The raw material components of the antistatic composite are 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide, and the mass ratio of the 90wt% ethanol solution, antistatic particles, sodium dodecylbenzene sulfonate, carboxymethyl cellulose and silicon dioxide is 86-90:18-22:3.7-4.3:3.0-3.4:8.3-8.

7.

7. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: The gluing step comprises applying glue to the dried surface wood chips and the dried core wood chips by mechanically mixing the adhesive, respectively, to obtain the glued surface wood chips and the glued core wood chips; The amount of glue applied on the surface layer is 2.5-3.0%, and the amount of glue applied is based on the mass ratio of absolute dry glue to absolute dry wood shavings; The glue application amount of the core layer is 2.1-2.5%, and the application amount is based on the mass ratio of absolute dry glue to absolute dry wood chips.

8. The method for preparing an antistatic oriented strand board according to claim 7, characterized in that: The preparation method of the adhesive comprises the following steps: mixing 32-37 g of isocyanate glue and 4.0-4.4 g of nano titanium dioxide, stirring evenly, adding 1.8-2.2 g of paraffin, 1.2-1.4 g of diacetyl tartaric acid monoglyceride and 1.6-1.8 g of sodium oleate for homogenization, wherein the homogenization time is 4.5-5.5 min and the homogenization pressure is 4.4-4.8 MPa. After the homogenization is completed, the adhesive is obtained.

9. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: The paving step comprises paving the glued core layer wood chips through a five-layer paving head to obtain a core layer material, and then paving the glued surface layer material on the upper and lower surfaces of the core layer material to obtain a slab; The core layer material is a three-layer structure, which is composed of a core layer upper surface layer, a core layer middle layer, and a core layer lower surface layer from top to bottom, wherein the core layer middle layer is paved horizontally, and the core layer upper surface layer and the core layer lower surface layer are paved vertically; When the surface material is paved, the surface wood chips after gluing are arranged longitudinally; The mass ratio of the core layer material to the surface layer material is 7.3-7.7:2.3-2.7; In the core layer material, the mass ratio of the core layer upper surface layer, the core layer middle layer, and the core layer lower surface layer is 1:0.8-1.2:1; The mass ratio of the upper layer to the lower layer of the surface material is 1:0.8-1.

2.

10. The method for preparing an antistatic oriented strand board according to claim 1, characterized in that: The hot pressing shaping step comprises: compacting the slab by a pre-pressing machine, and then cutting the slab into a required slab width by a slab trimming saw to obtain a sawn slab, and hot pressing the slab by a continuous flat press, and the hot pressing temperatures are 232-237°C, 218-224°C, 216-222°C, 198-202°C, and 167-173°C, respectively, the hot pressing factor is 5.8-6.2s / mm, and the pressures are 1.3-1.5MPa, 1.2-1.4MPa, 0.8-1.0MPa, 0.4-0.6MPa, and 0.7-0.9MPa, respectively. After the hot pressing is completed, a plain board is obtained.

Citation Information

Patent Citations

  • Environment-friendly graphene filament composite OSB oriented strand board pressed by using modified printed circuit board (PCB) resin fibers and graphene and preparation method of oriented strand board

    CN108424616A

  • Graphene oxide / zinc oxide antistatic polypropylene cast film

    CN111269493A

  • Geothermal special composite floor and preparation method thereof

    CN111393867A

  • Antistatic agent and preparation method thereof

    CN111996611A

  • Furniture skin-touch decorative film and preparation method thereof

    CN116496524A