Method for improving strength of 3D printing product
By adding curing agent and powdered sodium silicate solute to the 3D printing powder, using room temperature hardening and secondary drying technology, the microwave heating curing and silicate solute mass fraction limitations in inorganic binder jet 3D printing is solved. Problem, improving product strength and avoiding printhead clogging, expanding application range.
Patent Information
- Application Number
- CN202411191555.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing inorganic binder jet 3D printing technology requires microwave heating and curing and the mass fraction of silicate solute is limited, resulting in clogging and hardening of the print head, affecting product strength and application range.
Add 0.1%-2.0% curing agent, 0.1%-5.0% reinforcement and 1.0%-10% powdered sodium silicate solute to the 3D printing powder to improve product strength through room temperature hardening and secondary drying. Avoid microwave heating and improve silicate solute mass fraction.
It can improve product strength without microwave heating, avoid the problem of adhesive blocking the print head, enhance the strength and hygroscopicity of sodium silicate adhesive, and expand the application of inorganic adhesive in 3D sand printing potential.
Smart Images

Figure CN119077887A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of 3D printing, and in particular to a method for improving the strength of a binder jet 3D printed product. Background Art
[0002] Binder jet 3D printing technology is an additive manufacturing technology that can print three-dimensional products. With the development of this technology, it is widely used in the production of sand molds in the foundry field. This technology does not require mold opening to produce sand molds. Casting sand and binder are directly formed by 3D printing. At present, the main liquid binders used in binder jet 3D printing sand molds are furan resin, phenolic resin and inorganic binders. Among them, furan resin is widely used because of its fast molding speed, high strength and good surface quality at room temperature, but it releases formaldehyde during the molding process, which is not friendly to the environment and workers. Therefore, foundry companies began to seek inorganic binders that can replace furan resin to replace furan resin. The inorganic binders that are currently attracting attention are mainly silicates, but the binder needs microwave heating to cure after jet printing, and has disadvantages such as poor moisture absorption resistance and easy sand adhesion. In addition, the silicate inorganic binder used for binder jet 3D printing generally needs to control physical and chemical properties such as viscosity and surface tension to ensure that it is compatible with the print head. Therefore, the mass fraction of silicate solute as an enhancement will be limited to less than 30%. Increasing the inkjet volume will have problems with ink seepage and hardening difficulties, which limits the application of inorganic binders in 3D sand mold printing. Summary of the invention
[0003] Based on this, it is necessary to provide a method for improving the strength of 3D printed products to address the problems in the prior art that inorganic binders need to be cured by microwave heating after printing and that the print head nozzle is easily clogged when the mass fraction of the silicate binder solute is too high. This method does not require microwave heating and curing of the product green body after the product is printed, and can improve the strength of the printed product without increasing the mass fraction of the silicate solute added to the print head.
[0004] A method for improving the strength of a 3D printed product comprises the following steps:
[0005] Prepare a binder liquid material, and add a silicate inorganic binder into the print head;
[0006] Prepare mixed powder, mix 0.1%-2.0% of curing agent, 0.1%-5.0% of reinforcing agent, 1.0%-10% of powdered inorganic binder solute with powder material and add to sand spreader;
[0007] Print, set the printing parameters of the 3D printer and start printing the product green body;
[0008] Hardening: The green body of the printed product is first hardened at room temperature, and then sanded after reaching the sand cleaning strength, and the green body of the product after sand cleaning is hardened for the second time.
[0009] Furthermore, the powdered inorganic binder solute is a silicate powder solute.
[0010] Furthermore, the silicate inorganic binder is a sodium silicate inorganic binder.
[0011] Furthermore, the silicate powder solute is sodium silicate powder solute.
[0012] Furthermore, the modulus of the sodium silicate powder solute is 2.5-3.5.
[0013] Furthermore, the curing agent is an organic fat, and the viscosity of the curing agent is ≤50.0 mPa.s.
[0014] Furthermore, the reinforcing agent is a combination of one or more of silicon dioxide, aluminum oxide, and iron oxide.
[0015] Furthermore, the room temperature hardening includes: first hardening the printed product green body in a 3D printing work box at room temperature for 4-24 hours, moving the product green body out of the work box, cleaning the sand, and then continuing to harden in the air for 4-48 hours.
[0016] Furthermore, the secondary hardening includes: placing the product green body after room temperature hardening in a drying oven and continuing to dry it for 20-200 minutes.
[0017] Furthermore, during the secondary hardening, the temperature of the drying oven is 160° C.-200° C.
[0018] The present invention provides a method for improving the strength of 3D printed products, which adopts an inorganic sodium silicate binder. The sodium silicate binder is added to a print head, and a certain proportion of sodium silicate powder solute is evenly mixed into the printed powder. During printing, the sodium silicate powder solute is evenly laid layer by layer in a working box along with a powder spreader, and the print head sprays the binder on each layer of powder along with the powder spreader. Because a certain amount of sodium silicate powder solute is mixed into the powder, this part of the powder solute will combine with the liquid sodium silicate binder sprayed from the print head, and the powdered sodium silicate solute is miscible with the sodium silicate binder through subsequent room temperature hardening and secondary hardening treatment, thereby improving the strength of the binder, so that the green body after printing can reach the required product strength without microwave heating and curing; in addition, the mass fraction of the sodium silicate solute in the inorganic binder can be increased without increasing the mass fraction of the sodium silicate solute in the print head, thereby improving the strength of the binder, and preventing the binder from clogging the nozzle of the print head. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1The present invention is a flow chart of a method for improving the strength of 3D printed products. DETAILED DESCRIPTION
[0020] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0021] It should be noted that when an element is referred to as being "disposed on" another element, it may be directly on the other element or there may be a centered element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a centered element at the same time. The terms "vertical", "horizontal", "left", "right", "top", "bottom", "bottom end", "top end" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0023] The present invention provides a method for improving the strength of a 3D printed product, comprising the following steps:
[0024] Prepare a binder metallurgy, and add a silicate inorganic binder into the print head;
[0025] Prepare mixed powder, mix 0.1%-2.0% of curing agent, 0.1%-5.0% of reinforcing agent, 1.0%-10% of powdered inorganic binder solute with powder material and add to sand spreader;
[0026] Print, set the printing parameters of the 3D printer and start printing the product green body;
[0027] Hardening: The green body of the printed product is first hardened at room temperature, and then sanded after reaching the sand cleaning strength, and the green body of the product after sand cleaning is hardened for the second time.
[0028] The present invention provides a method for improving the strength of 3D printed products. The method comprises the following steps: mixing a certain amount of silicate powder solute into the printing powder, and replenishing the silicate solute without increasing the mass fraction of the silicate solute in the binder liquid. After the powdered silicate solute is spread by the powder spreader, the powdered silicate solute will combine with the liquid silicate binder sprayed from the print head, and will be miscible with the liquid silicate binder in the subsequent room temperature hardening and secondary hardening treatment processes, thereby improving the strength of the binder. The printed green body does not need to be cured by microwave heating, and only conventional hardening is required to achieve the strength required by the product.
[0029] The method for improving the strength of a 3D printed product is described below with reference to a specific example, so as to further understand the inventive concept of improving the strength of a 3D printed product.
[0030] like Figure 1 As shown, a method for improving the strength of a 3D printed product comprises the following steps:
[0031] Prepare a binder liquid and add a silicate inorganic binder to a print head. Specifically, add the silicate inorganic binder to the ink supply box of the print head of the 3D printing device. During the printing process, the silicate inorganic binder is sprayed onto the powder surface through the print head. The viscosity of the sodium silicate binder is 5.0-20.0 mPs·s and the density is 0.8-1.5 g / cm 3 , pH is 7.0-14.0.
[0032] Prepare mixed powder, mix 0.1%-2.0% curing agent, 0.1%-5.0% reinforcing agent, 1.0%-10% powdered inorganic binder solute with powder material and add to the sand spreader. Among them, 0.1%-2.0% is the mass fraction of curing agent in powder material, 0.1%-5.0% is the mass fraction of reinforcing agent in powder material, and 1.0%-10% is the mass fraction of powdered inorganic binder in powder material. When preparing mixed powder, set the sand mixing parameters and sand mixing sequence, the sand mixing tank automatically absorbs sand, set the sand mixing time to 30-100s, first add 0.1-2.0 curing agent and mix for 20-40s, then add 0.1%-5.0% powder reinforcing agent and 1.0%-10% powdered silicate solute and mix evenly for use in the sand spreader. The modulus of the powdered sodium silicate solute is 3; the curing agent is preferably liquid triacetin, with a viscosity of ≤50.0 mPs·s and a density of 0.8-1.5 g / cm 3 , pH is 5-10. The particle size range of the powder enhancer is 5-200μm.
[0033] Print, set the printing parameters of the 3D printer, and start printing the green product. Specifically, the sand spreader first spreads the powder, and the print head sprays the binder liquid on each layer of powder along with the sand spreader, and this cycle continues until the green product is printed.
[0034] Hardening: The green body of the product after printing is first hardened at room temperature, and then sanded after reaching the sand cleaning strength, and the green body of the product after sand cleaning is hardened for the second time. That is, after the green body of the product is printed, do not move it out of the working box first, and let the green body of the product harden at room temperature in the working box for a period of time. After reaching the strength required for sand cleaning, open the working box, clean the green body of the product, and then harden the green body after sand cleaning for the second time to achieve the final required strength of the product.
[0035] Preferably, the powdered inorganic binder solute is a silicate powder solute.
[0036] Preferably, the silicate inorganic binder is a sodium silicate inorganic binder.
[0037] Preferably, the silicate powder solute is sodium silicate powder solute, and the modulus of the sodium silicate powder solute is 2.5-3.5.
[0038] Preferably, the curing agent is an organic fat, and the viscosity of the curing agent is ≤50.0 mPa.s.
[0039] Preferably, the reinforcing agent is a combination of one or more of silicon dioxide, aluminum oxide and iron oxide.
[0040] Preferably, the room temperature hardening includes: first hardening the printed product green body in a 3D printing work box at room temperature for 4-24 hours, moving the product green body out of the work box, cleaning the sand, and then continuing to harden in the air for 4-48 hours.
[0041] Preferably, the secondary hardening comprises: placing the product green body after room temperature hardening in a drying oven and continuing to dry it for 20-200 minutes.
[0042] Preferably, the temperature of the drying oven during secondary hardening is 160°C-200°C.
[0043] The method for improving the strength of a 3D printed product of the present invention does not need to increase the mass fraction of an inorganic binder in a print head. By adding a powdered inorganic binder solute into a powder material, the powdered inorganic binder solute will combine with a liquid inorganic binder ejected from the print head. In subsequent room temperature hardening and secondary hardening, the powdered inorganic binder solute will be miscible with the liquid inorganic binder, thereby increasing the mass fraction of the inorganic binder solute, further increasing the strength of the printed product, and this method will not clog the nozzle of the print head.
[0044] Embodiment 1:
[0045] Prepare the binder liquid, add the inorganic sodium silicate binder into the ink supply box of the print head for use. The viscosity of the sodium silicate binder is 5.0-20.0mPs·s and the density is 0.8-1.5g / cm 3 , pH is 7.0-14.0.
[0046] Prepare the mixed powder, mix 100-140 mesh casting sand with 0.4% curing agent, then add 0.6% powdered reinforcing agent and 5% sodium silicate powder and mix them evenly for use. The modulus of the powdered sodium silicate solute is 3; the curing agent is liquid triacetin curing agent, the viscosity of which is ≤50.0mPs·s and the density is 0.8-1.5g / cm 3 , pH is 5-10. The particle size range of the powder enhancer is 5-200μm.
[0047] Printing, add the mixed powder into the sanding device of the printer, set the printing parameters and start printing. The printing process is shown in Table 1:
[0048] Table 1 Printing parameters
[0049]
[0050] hardening:
[0051] Room temperature hardening: After printing, the sand mold is first hardened in the working box at room temperature for 8 hours and then the sand is cleaned. The sand mold after sand cleaning continues to harden in the air for 40 hours;
[0052] Secondary hardening: Move the sand mold to a blast drying oven and continue drying for 30 minutes to allow the sand mold to reach its final strength.
[0053] Table 2 Performance comparison
[0054]
[0055] From the comparative experiment in Table 2, it can be seen that after mixing powdered sodium silicate solute into the powder, the average compressive strength of the final sand mold is significantly improved.
[0056] Embodiment 2:
[0057] Prepare the binder liquid, add the inorganic sodium silicate binder into the ink supply box of the print head for standby use; wherein the viscosity of the sodium silicate binder is 5.0-20.0mPs·s and the density is 0.8-1.5g / cm 3 , pH is 7.0-14.0.
[0058] Prepare the mixed powder, mix 100-140 mesh casting sand with 0.3% curing agent, then add 0.4% powdered reinforcing agent and 3% sodium silicate powder and mix them evenly for use. The modulus of the powdered sodium silicate solute is 3; the curing agent is liquid triacetin curing agent, the viscosity of which is ≤50.0mPs·s and the density is 0.8-1.5g / cm 3 , pH is 5-10. The particle size range of the powder enhancer is 5-200μm.
[0059] Printing, add the mixed powder into the sanding device of the printer, set the printing parameters and start printing. The printing process is shown in Table 3:
[0060] Table 1 Printing parameters
[0061]
[0062] hardening:
[0063] Room temperature hardening: After printing, the sand mold is first hardened in the working box at room temperature for 8 hours and then the sand is cleaned. The sand mold after sand cleaning continues to harden in the air for 40 hours;
[0064] Secondary hardening: Move the sand mold to a blast drying oven and continue drying it at 160°C for 100 minutes to allow the sand mold to reach its final strength.
[0065] Table 4 Performance comparison
[0066]
[0067] From the comparative experiments in Table 4, it can be seen that after the powdered sodium silicate solute is mixed into the powder, the average compressive strength of the final sand mold is significantly improved.
[0068] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0069] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for improving the strength of a 3D printed product, characterized in that: The method for improving the strength of 3D printed products comprises the following steps: Prepare a binder liquid material, and add a silicate inorganic binder into the print head; Prepare mixed powder, mix 0.1%-2.0% of curing agent, 0.1%-5.0% of reinforcing agent, 1.0%-10% of powdered inorganic binder solute with powder material and add to sand spreader; Print, set the printing parameters of the 3D printer and start printing the product green body; Hardening: The green body of the printed product is first hardened at room temperature, and then sanded after reaching the sand cleaning strength, and the green body of the product after sand cleaning is hardened for the second time.
2. A method for improving the strength of 3D printed products according to claim 1, characterized in that: The powdered inorganic binder solute is a silicate powder solute.
3. A method for improving the strength of 3D printed products according to claim 1, characterized in that: The silicate inorganic binder is a sodium silicate inorganic binder.
4. A method for improving the strength of 3D printed products according to claim 2, characterized in that: The silicate powder solute is sodium silicate powder solute.
5. A method for improving the strength of 3D printed products according to claim 4, characterized in that: The modulus of the sodium silicate powder solute is 2.5-3.
5.
6. A method for improving the strength of 3D printed products according to claim 1, characterized in that: The curing agent is organic fat, and the viscosity of the curing agent is ≤50.0 mPa·s.
7. A method for improving the strength of 3D printed products according to claim 1, characterized in that: The reinforcing agent is a combination of one or more of silicon dioxide, aluminum oxide and iron oxide.
8. A method for improving the strength of 3D printed products according to claim 1, characterized in that: The room temperature hardening includes: first hardening the printed product green body in a 3D printing work box at room temperature for 4-24 hours, removing the product green body from the work box, cleaning the sand, and then continuing to harden in the air for 4-48 hours.
9. A method for improving the strength of 3D printed products according to claim 1, characterized in that: The secondary hardening includes: placing the product green body after room temperature hardening in a drying oven and continuing to dry it for 20-200 minutes.
10. A method for improving the strength of 3D printed products according to claim 9, characterized in that: During secondary hardening, the temperature of the drying oven is 160°C-200°C.