Para-aramid honeycomb, temperature-resistant honeycomb core material and preparation method thereof
By using polyimide node glue and ultraviolet curing technology, as well as the method of composite with phthalene resin, the high temperature resistance of aramid honeycombs is improved, and the resistance of missile head radome material at ultra-high temperatures is solved. The problem of insufficient temperature performance achieves excellent dielectric performance and high heat resistance in 500℃ environment.
Patent Information
- Application Number
- CN202411229995.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
The existing aramid honeycomb core material cannot meet the ultra-high temperature requirements of the missile head radome under high Mach flight conditions, and its temperature resistance is insufficient.
Para-aramid honeycombs are prepared by polyimide node glue and ultraviolet curing technology, and are combined with phthalonitrile resin to improve the high temperature resistance of the material through tensile setting and glue-impregnation curing processes.
After insulated at 500℃ for 10 minutes, the material maintains excellent dielectric properties, with a dielectric constant of 0.9~1.3, a dielectric loss ≤1.5×10-2, and a heat resistance is increased to 300℃, which is insoluble in acetone, etc. Organic solvent.
Smart Images

Figure BDA0005025819650000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of high-temperature resistant and wave-transmitting composite materials, and in particular relates to a para-aramid honeycomb, a temperature-resistant honeycomb core material and a preparation method thereof. Background Art
[0002] Aramid honeycomb core materials are widely used in radar antenna covers as dielectric matching materials. Under normal circumstances, the existing meta- or para-aramid honeycomb core materials can meet the temperature requirements of the use environment. However, for missile head antenna covers, under high Mach flight conditions, the material's temperature resistance is required to be high. The existing aramid honeycomb core materials are limited by the node glue and resin matrix. The development idea of conventional heat-resistant honeycombs is mainly to find ways to replace the heat-resistant node glue. The temperature resistance target of the heat-resistant honeycomb design is generally 350℃~400℃, which cannot meet this ultra-high temperature requirement.
[0003] For example, a Chinese patent document with publication number CN118223291A discloses a method for preparing a high-temperature resistant aramid honeycomb that can be used for a long time at 250°C. The high-temperature stability of the aramid honeycomb is improved by adding high-temperature resistant aerogel particles to the impregnation liquid during the aramid honeycomb forming process and covering the aerogel particles on the surface of the aramid honeycomb. In addition, this method only requires adding the prepared aerogel particles to the impregnation liquid during the honeycomb forming process, without adding new steps, with a short cycle and a simple method, which provides technical support for the industrial preparation of high-temperature resistant aerogel coatings. However, the temperature resistance target of the heat-resistant honeycomb design is generally 350°C to 400°C, which cannot meet the requirements of such ultra-high temperatures.
[0004] Therefore, under the condition of ensuring the dielectric properties of the material, improving the temperature resistance of aramid honeycomb has very important significance and application prospects. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a para-aramid honeycomb, a heat-resistant honeycomb core material and a preparation method thereof, aiming to solve the problem of poor heat resistance of the aramid honeycomb under the condition of ensuring the dielectric properties of the material.
[0006] In order to solve the above problems, the first aspect of the present invention provides a method for preparing a para-aramid honeycomb, comprising the following steps:
[0007] S1. Coating a node glue on the surface of the para-aramid paper, and then stacking multiple layers of para-aramid paper coated with node glue, and finally UV curing to obtain an aramid paper laminate, wherein the node glue is a polyimide node glue;
[0008] S2. The aramid paper stack is stretched and shaped to obtain a honeycomb block;
[0009] S3. The honeycomb block is impregnated and cured to obtain a para-aramid paper honeycomb block;
[0010] S4. Slicing the para-aramid paper honeycomb block to obtain the para-aramid honeycomb.
[0011] Preferably, in step S1, during UV curing, the distance between the UV light source and the node glue is 10 to 15 cm, the current flux of the UV light source is 100%, and the curing time is 30 to 35 min; in step S2, the temperature during stretching and shaping is 100 to 105°C, and the heat preservation is 35 to 60 min; in step S3, the impregnating resin used for curing after dipping is barium phenolic resin, the curing temperature is 170 to 175°C, and the heat preservation is 120 to 125 min.
[0012] The second aspect of the present invention provides a para-aramid honeycomb prepared by the above-mentioned preparation method.
[0013] The third aspect of the present invention provides a temperature-resistant honeycomb core material, comprising:
[0014] The para-aramid honeycomb and the phthalonitrile resin composited with the para-aramid honeycomb as mentioned above; the mass ratio of the para-aramid honeycomb to the phthalonitrile resin is 10-15:1.
[0015] Preferably, the density of the honeycomb core material is 35-45 kg / m 3 .
[0016] Preferably, the dielectric constant of the honeycomb core material is 0.9 to 1.3 after being kept at 500°C for 10 minutes, and the dielectric loss is ≤1.5×10 -2 .
[0017] A fourth aspect of the present invention provides a method for preparing the above-mentioned temperature-resistant honeycomb core material, comprising the following steps:
[0018] A1: mixing phthalonitrile resin and solvent to obtain resin glue;
[0019] A2: dipping the para-aramid honeycomb into the resin glue and then drying it;
[0020] A3: Curing the air-dried para-aramid honeycomb to obtain the temperature-resistant honeycomb core material.
[0021] Preferably, in step A1, the solvent is acetone, and the mass ratio of the phthalonitrile resin to the solvent is 1:4-6.
[0022] Preferably, in step A1, the mixing of the phthalonitrile resin and the solvent is carried out by a cantilever constant speed powerful electric stirrer, with a rotation speed of 800 to 1000 r / min and a mixing time of 100 to 120 s.
[0023] Preferably, in step A3, the curing system of the para-aramid honeycomb is: heating to 80±5°C and keeping warm for 60±5min; heating from 80±5°C to 150±5°C and keeping warm for 60±5min; heating from 150±5°C to 300±5°C and keeping warm for 180±5min; heating from 300±5°C to 400±5°C and keeping warm for 60±5min; heating from 400±5°C to 500±5°C and keeping warm for 10±5min, with a heating rate of 5 to 10°C / min.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The para-aramid honeycomb of the present invention uses a more heat-resistant polyimide node glue, is prepared and molded by ultraviolet pre-curing, and does not swell or dissolve in various solvents such as acetone; existing commercial products are all phenolic or epoxy node glues, which meet the curing process below 260°C, but cannot withstand the 316°C post-treatment process, have low heat resistance, and are only 150°C in the long term. In addition, the phenolic or epoxy node glues will dissolve in organic solvents such as acetone, while the polyimide node glue used in the present invention is heat-resistant, with a long-term heat resistance of 300°C, high heat resistance, and does not dissolve in various organic solvents such as acetone. The high-temperature resistant honeycomb core material prepared by the present invention not only has low density and can withstand 500°C high temperature for 10 minutes, but also can maintain excellent material dielectric properties. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] A first aspect of an embodiment of the present invention provides a method for preparing a para-aramid honeycomb, comprising the following steps:
[0028] S1. Coating a node glue on the surface of the para-aramid paper, and then stacking multiple layers of para-aramid paper coated with node glue, and finally UV curing to obtain an aramid paper laminate, wherein the node glue is a polyimide node glue;
[0029] S2. The aramid paper stack is stretched and shaped to obtain a honeycomb block;
[0030] S3. The honeycomb block is impregnated and cured to obtain a para-aramid paper honeycomb block;
[0031] S4. Slicing the para-aramid paper honeycomb block to obtain the para-aramid honeycomb.
[0032] The para-aramid honeycomb of the embodiment of the present invention uses a more heat-resistant polyimide node glue, is prepared and formed by ultraviolet pre-curing, and does not swell or dissolve in various solvents such as acetone; the existing commercial products are all phenolic or epoxy node glues, which meet the curing process below 260°C, but cannot withstand the 316°C post-treatment process, have low heat resistance, and are only 150°C in the long term. The phenolic or epoxy node glue will dissolve in organic solvents such as acetone, while the polyimide node glue used in the present invention is resistant to high temperatures, with a long-term heat resistance of 300°C, high heat resistance, and does not dissolve in various organic solvents such as acetone; ultraviolet curing can save resources and eliminate heating equipment such as ovens. The high-temperature resistant honeycomb core material prepared by the present invention not only has low density and can withstand 500°C high temperature for 10 minutes, but also can maintain excellent material dielectric properties.
[0033] In some embodiments, in step S1, during UV curing, the distance between the UV light source and the node glue is 10 to 15 cm, the current flux of the UV light source is 100%, and the curing time is 30 to 35 minutes; in step S2, the temperature during stretching and shaping is 100 to 105°C, and the heat preservation is 35 to 60 minutes; in step S3, the impregnating resin used for curing after dipping is barium phenolic resin, the curing temperature is 170 to 175°C, and the heat preservation is 120 to 125 minutes.
[0034] A second aspect of the embodiments of the present invention provides a para-aramid honeycomb prepared by the above-mentioned preparation method.
[0035] A third aspect of an embodiment of the present invention provides a temperature-resistant honeycomb core material, comprising:
[0036] The para-aramid honeycomb and the phthalonitrile resin composited with the para-aramid honeycomb as mentioned above; the mass ratio of the para-aramid honeycomb to the phthalonitrile resin is 10-15:1.
[0037] The heat-resistant honeycomb core material of the embodiment of the present invention adopts a para-aramid honeycomb prepared with polyimide node glue as the reinforcement material, which is resistant to high temperatures and has a long-term heat resistance of 300°C. It has high heat resistance and is insoluble in various organic solvents such as acetone. The resin matrix adopts phthalonitrile resin, which can withstand high temperatures above 500°C and has excellent solubility and dispersibility.
[0038] In some embodiments, the density of the honeycomb core material is 35-45 kg / m 3 .
[0039] In some embodiments, the dielectric constant of the honeycomb core material is 0.9 to 1.3 after being kept at 500°C for 10 minutes, and the dielectric loss is ≤1.5×10 -2 .
[0040] A fourth aspect of an embodiment of the present invention provides a method for preparing the above-mentioned temperature-resistant honeycomb core material, comprising the following steps:
[0041] A1: mixing phthalonitrile resin and solvent to obtain resin glue;
[0042] A2: dipping the para-aramid honeycomb into the resin glue and then drying it;
[0043] A3: Curing the air-dried para-aramid honeycomb to obtain the temperature-resistant honeycomb core material.
[0044] Preferably, in step A1, the solvent is acetone, and the mass ratio of phthalonitrile resin to solvent is 1:4-6. Such a mass ratio of resin to solvent can ensure that the density of the honeycomb core material is maintained at 35-45 kg / m 3 .
[0045] In some embodiments, in step A1, the mixing of the phthalonitrile resin and the solvent is performed by a cantilever constant speed powerful electric stirrer, with a rotation speed of 800 to 1000 r / min and a mixing time of 100 to 120 s.
[0046] In some embodiments, in step A3, the curing system of the para-aramid honeycomb is: heating to 80±5°C and keeping warm for 60±5min; heating from 80±5°C to 150±5°C and keeping warm for 60±5min; heating from 150±5°C to 300±5°C and keeping warm for 180±5min; heating from 300±5°C to 400±5°C and keeping warm for 60±5min; heating from 400±5°C to 500±5°C and keeping warm for 10±5min, with a heating rate of 5 to 10°C / min.
[0047] Example 1
[0048] The heat-resistant honeycomb core material of this embodiment includes:
[0049] The prepared cell side length is 2mm and the density is 40kg / m 3 , 2mm thick regular hexagonal honeycomb core material with a temperature resistance of 500℃.
[0050] The method for preparing the para-aramid honeycomb of this embodiment comprises the following steps:
[0051] S1. Select a domestic para-aramid honeycomb core strip with a grade of AC-KH and a thickness of 2 mm as a reinforcing material for the honeycomb core material, coat the surface of the para-aramid paper with polyimide node glue, then stack multiple layers of para-aramid paper coated with node glue, and finally use ultraviolet curing to obtain an aramid paper laminate. The distance between the ultraviolet light source and the node glue is 10 cm, and the current flux of the ultraviolet light source is set to 100% to ensure sufficient light intensity for the curing reaction. The curing time is 30 minutes;
[0052] S2. The aramid paper laminate is stretched, and when the honeycomb cells reach the size required by the process, the stretched honeycomb is fixed on a tool and placed in an oven for shaping to obtain a honeycomb block; the temperature during the stretching and shaping in the oven is 100°C, and the temperature is kept for 1h;
[0053] S3. The unimpregnated honeycomb block was impregnated in barium phenolic resin and then cured at a curing temperature of 170 ° C for 2 h to obtain a para-aramid paper honeycomb block;
[0054] S4. Slice the para-aramid paper honeycomb block into 2 mm thick honeycomb materials to obtain the para-aramid honeycomb.
[0055] The method for preparing the heat-resistant honeycomb core material of this embodiment comprises the following steps:
[0056] A1: Select high temperature resistant thermoplastic phthalonitrile resin with the grade of 20240416-A as the impregnation resin of the honeycomb core material, select acetone as the oily solvent of the phthalonitrile resin, prepare the phthalonitrile resin and acetone solution at a mass ratio of 1:5, mix them evenly with a cantilever constant speed strong electric stirrer, the speed is 800r / min, the mixing time is 2min, and the mixture is placed in an impregnation container;
[0057] A2: The size of the aramid honeycomb is 50*50*2mm. Fix the prepared aramid honeycomb core material on the metal frame, hold the metal frame handle, and immerse the front and back sides in the dipping container; after dipping, use a fan to blow out the glue in the holes and place it in a ventilated environment to dry;
[0058] A3: Place the dried honeycomb in an oven, naturally heat it from room temperature to 80°C, keep it warm for 1 hour, then heat it from 80°C to 150°C, keep it warm for 1 hour, then heat it from 150°C to 300°C, keep it warm for 3 hours, then heat it from 300°C to 400°C, keep it warm for 1 hour, and finally heat it from 400°C to 500°C, keep it warm for 10 minutes, and the heating rate is 5°C / min. A heat-resistant honeycomb core material is obtained.
[0059] The measured density of the material is 43kg / m 3 , the dielectric constant is 1.01, and the dielectric loss is 8.1×10 -3 , the flat compressive strength is 2.5MPa.
[0060] Comparative Example 1
[0061] The difference between this comparative example and Example 1 is that the para-aramid honeycomb is prepared by using phenolic resin node glue.
[0062] The measured density of the material is 43kg / m 3 , the dielectric constant is 1.01, and the dielectric loss is 8.1×10 -3 . The flat compressive strength is 2.0MPa.
[0063] Comparative Example 2
[0064] The difference between this comparative example and Example 1 is that the para-aramid honeycomb is prepared by using epoxy resin node glue.
[0065] The measured density of the material is 43kg / m 3 , the dielectric constant is 1.01, and the dielectric loss is 8.1×10 -3 . The flat compressive strength is 2.3MPa.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 1 is that the para-aramid honeycomb is not cured by ultraviolet light but cured by heating.
[0068] The measured density of the material is 43kg / m 3 , the dielectric constant is 1.01, and the dielectric loss is 8.1×10 -3 . The flat compressive strength is 2.4MPa.
[0069] Comparative Example 4
[0070] The difference between this comparative example and Example 1 is that a high temperature resistant thermoplastic polyimide resin with a grade of KHTC-320 is selected as the impregnation resin of the honeycomb core material, and diethylene glycol dimethyl ether is selected as the oily solvent; the polyimide resin and diethylene glycol dimethyl ether solution are prepared in a mass ratio of 1:1.5.
[0071] The measured density of the material is 40kg / m 3 , the dielectric constant is 1.14, and the dielectric loss is 1.2×10 -2 . The flat compressive strength is 2.0MPa.
[0072] Comparative Example 5
[0073] The difference between this comparative example and Example 1 is that the phthalonitrile resin and the acetone solution are prepared in a mass ratio of 1:6.
[0074] The measured density of the material is 40kg / m 3 , the dielectric constant is 1.07, and the dielectric loss is 8.5×10 -3. The flat compressive strength is 2.2MPa.
[0075] Table 1 Comparison of relevant data of various embodiments and comparative examples
[0076]
[0077] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a para-aramid honeycomb, characterized in that: The steps include: S1. Coating a node glue on the surface of the para-aramid paper, and then stacking multiple layers of para-aramid paper coated with node glue, and finally UV curing to obtain an aramid paper laminate, wherein the node glue is a polyimide node glue; S2. The aramid paper stack is stretched and shaped to obtain a honeycomb block; S3. The honeycomb block is impregnated and cured to obtain a para-aramid paper honeycomb block; S4. Slicing the para-aramid paper honeycomb block to obtain the para-aramid honeycomb.
2. The method for preparing a para-aramid honeycomb according to claim 1, characterized in that: In step S1, during UV curing, the distance between the UV light source and the node glue is 10 to 15 cm, the current flux of the UV light source is 100%, and the curing time is 30 to 35 minutes; in step S2, the temperature during stretching and shaping is 100 to 105° C., and the temperature is kept for 35 to 60 minutes; in step S3, the impregnating resin used during curing after dipping is barium phenolic resin, the curing temperature is 170 to 175° C., and the temperature is kept for 120 to 125 minutes.
3. A para-aramid honeycomb prepared by the preparation method according to claim 1 or 2.
4. A temperature-resistant honeycomb core material, characterized in that: include: The para-aramid honeycomb as claimed in claim 3 and the phthalonitrile resin composited with the para-aramid honeycomb; the mass ratio of the para-aramid honeycomb to the phthalonitrile resin is 10 to 15:
1.
5. The heat-resistant honeycomb core material according to claim 4, characterized in that: The density of honeycomb core material is 35~45kg / m 3 .
6. The heat-resistant honeycomb core material according to claim 4, characterized in that: The dielectric constant of the honeycomb core material is 0.9-1.3 after being kept at 500℃ for 10 minutes, and the dielectric loss is ≤1.5×10 -2 .
7. A method for preparing a heat-resistant honeycomb core material according to any one of claims 4 to 6, characterized in that: The steps include: A1: mixing phthalonitrile resin and solvent to obtain resin glue; A2: dipping the para-aramid honeycomb into the resin glue and then drying it; A3: Curing the air-dried para-aramid honeycomb to obtain the temperature-resistant honeycomb core material.
8. The method for preparing the heat-resistant honeycomb core material according to claim 7, characterized in that: In step A1, the solvent is acetone, and the mass ratio of the phthalonitrile resin to the solvent is 1:4-6.
9. The method for preparing the heat-resistant honeycomb core material according to claim 7, characterized in that: In step A1, the phthalonitrile resin and the solvent are mixed by a cantilever constant speed powerful electric stirrer, with a rotation speed of 800 to 1000 r / min and a mixing time of 100 to 120 s.
10. The method for preparing the heat-resistant honeycomb core material according to claim 7, characterized in that: In step A3, the curing system of the para-aramid honeycomb is as follows: heating to 80±5°C and keeping warm for 60±5min; heating from 80±5°C to 150±5°C and keeping warm for 60±5min; heating from 150±5°C to 300±5°C and keeping warm for 180±5min; heating from 300±5°C to 400±5°C and keeping warm for 60±5min; heating from 400±5°C to 500±5°C and keeping warm for 10±5min, with a heating rate of 5 to 10°C / min.
Citation Information
Patent Citations
High-temperature-resistant honeycomb core material and preparation method thereof
CN109677014A
Method for preparing light flexible high-temperature resistance honeycomb core material
CN111421898A
High-temperature composite honeycomb
CN114126852A
Castor oil modified photocuring wave-absorbing coating and preparation method thereof, honeycomb sandwich wave-absorbing material and preparation method thereof
CN114686097A
High-temperature-resistant carbon fiber paper, honeycomb core material and preparation method of honeycomb core material