Basalt fiber reinforced CPI resin mobile phone cover plate and preparation method thereof
By forming an adhesive layer and a basalt fiber-reinforced CPI resin layer on the ceramic substrate, the problems of high density and high cost of ceramic mobile phone covers are solved, and a thinner and high-performance mobile phone covers are achieved.
Patent Information
- Application Number
- CN202410990731.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing ceramic mobile phone cover has high density and high brittleness, resulting in heavier weight and high cost, which limits its use in the mobile phone cover field.
The strength and toughness of the mobile phone cover plate are improved and its thickness is reduced to achieve lightness by forming an adhesive layer and a basalt fiber reinforced CPI resin layer on the ceramic substrate.
It realizes a mobile phone cover with low density, light weight, high strength and good toughness, which reduces the use of ceramic materials, reduces costs, and improves impact resistance and connection firmness.
Smart Images

Figure BDA0004958796440000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of mobile phone cover plates, and in particular to a mobile phone cover plate of basalt fiber reinforced CPI resin and a preparation method thereof. Background Art
[0002] At present, mobile phone covers are mainly made of plastic, metal, glass and ceramic materials. Among them, the plastic (polycarbonate) cover has good comprehensive performance, but its wear resistance, heat dissipation, body feel are poor, and it is easy to age. It is mainly used in low-end and mid-end mobile phones; metal cover has the advantages of anti-fall, strong plasticity, and good heat dissipation, and has become the standard of mainstream mobile phones. With the advent of the era of 5G networks and wireless charging, smartphones have higher and higher requirements for signal transmission. The metal cover has a greater signal shielding effect, which has become a key factor restricting its development. Therefore, the material of mobile phone covers will inevitably change from metal covers to non-electromagnetic shielding materials such as glass and ceramics. Because the bending strength, hardness, wear resistance and heat dissipation of ceramic covers are better than those of glass covers, they have become an important choice for mobile phone manufacturers to achieve material differentiation of mobile phones. At present, the ceramic materials used to make mobile phone covers are mainly zirconium oxide, aluminum oxide, silicon carbide, etc. Among them, zirconium oxide is the most widely used ceramic material in mobile phone covers.
[0003] However, ceramic materials are dense and brittle. In order to improve the impact resistance of ceramic mobile phone covers, ceramic products are often thicker, resulting in heavier weight. For example, the relative density of zirconia ceramics (with the density of water at 4°C as the reference density) reaches 6.0, and the weight of its products is relatively large, which has become a widely criticized point for its use as mobile phone covers. In addition, heavier products will inevitably consume more expensive ceramic powders, which in turn leads to higher costs, limiting its use in the field of mobile phone covers. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a basalt fiber reinforced CPI resin mobile phone cover and a preparation method thereof, wherein the mobile phone cover has the advantages of low density, light weight, high strength, good toughness and low cost.
[0005] The invention provides a basalt fiber reinforced CPI resin mobile phone cover plate, which comprises a ceramic substrate, an adhesive layer and a basalt fiber reinforced CPI resin layer.
[0006] In the present invention, an adhesive layer and a basalt fiber reinforced CPI resin layer are sequentially arranged on a ceramic substrate to form a mobile phone cover. While reducing the use of ceramic materials, the basalt fiber reinforced CPI resin layer has high strength and good toughness, thereby improving the overall strength and toughness of the mobile phone cover, and reducing the thickness of the mobile phone cover while meeting the strength requirement, thereby achieving lightness and thinness.
[0007] Preferably, the adhesive layer is formed by coating an alcohol aqueous solution of a silane coupling agent on a ceramic substrate and then curing it;
[0008] Preferably, the silane coupling agent is at least one of KH-550, KH-560, KH-570 or KH-580.
[0009] In the present invention, in order to improve the adhesion between the ceramic substrate and the basalt fiber reinforced CPI resin layer, an alcohol aqueous solution of a silane coupling agent is coated on the ceramic substrate and cured to form a binder layer. As a strong chemical bond is formed between the silane coupling agent and the oxygen-containing groups on the surface of the ceramic substrate, when a basalt fiber cloth pre-impregnated with a CPI resin glue is subsequently applied, the binder layer of the silane coupling agent can form a strong chemical bond with the basalt fiber reinforced CPI resin layer, thereby enhancing the adhesion between the basalt fiber reinforced CPI resin layer and the ceramic substrate, and finally allowing the basalt fiber reinforced CPI resin layer to be better attached to the ceramic substrate, thereby obtaining a mobile phone cover with excellent performance.
[0010] Preferably, the basalt fiber reinforced CPI resin layer is formed by hot pressing and curing a basalt fiber cloth pre-impregnated with CPI resin glue.
[0011] Preferably, the CPI resin glue is a fluorinated polyimide resin glue;
[0012] Preferably, the fluorinated polyimide resin glue is obtained by copolymerizing a fluorinated diamine monomer and a non-fluorinated dianhydride monomer or a fluorinated dianhydride monomer in an organic solvent;
[0013] Preferably, the fluorine-containing diamine monomer is at least one of 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether, 2,2′-bis(trifluoromethyl)-4,4′-diaminobiphenyl, 2,2-bis-(3-amino-4-hydroxyphenyl)hexafluoropropane or tetrafluoro-metaphenylenediamine; the dianhydride monomer is at least one of 4,4′-(hexafluoroisopropylene)diphthalic anhydride, 1,2,4,5-cyclohexanetetracarboxylic anhydride, 1,2,3,4-cyclobutanetetracarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic anhydride or pyromellitic anhydride.
[0014] Preferably, the basalt fiber cloth is further immersed in an aqueous solution containing hexadecyltrimethylammonium bromide before being pre-impregnated with the CPI resin glue.
[0015] In the present invention, after the basalt fiber cloth is immersed in an aqueous solution containing hexadecyltrimethylammonium bromide before being pre-impregnated with CPI resin glue, the hexadecyltrimethylammonium bromide can form an intercalation layer in the pores on the surface of the basalt fiber cloth or in the interlayer gaps, thereby being grafted on the surface of the basalt fiber cloth. Then, the CPI resin glue is a fluorine-containing polyimide resin glue, and there are fluorine-containing polar groups in its molecular chain. In this way, when the basalt fiber cloth is pre-impregnated with the CPI resin glue, the basalt fiber cloth with hexadecyltrimethylammonium bromide grafted on the surface can adsorb the CPI resin glue, so that the CPI resin glue is firmly attached to the surface of the basalt fiber cloth, ensuring the stability of the CPI resin coating in the basalt fiber cloth, improving the flexural and tensile properties of the basalt fiber, and also helping to make the basalt fiber reinforced CPI resin layer better attached to the ceramic substrate.
[0016] Preferably, the ceramic substrate is at least one of a zirconium oxide ceramic substrate, an aluminum oxide ceramic substrate or a silicon carbide ceramic substrate.
[0017] Preferably, the thickness of the ceramic substrate is 0.1-1 mm, the thickness of the adhesive layer is 5-50 μm, and the thickness of the fiber-reinforced resin layer is 0.1-1 mm.
[0018] The present invention also provides a method for preparing the basalt fiber reinforced CPI resin mobile phone cover, comprising the following steps:
[0019] S1. providing a ceramic substrate;
[0020] S2, coating the ceramic substrate with an alcohol aqueous solution of a silane coupling agent, and forming a binder layer after curing;
[0021] S3, pasting basalt fiber cloth pre-impregnated with CPI resin glue on the adhesive layer, and forming a basalt fiber reinforced CPI resin layer after hot pressing and curing to obtain the mobile phone cover.
[0022] Preferably, in step S2, in the alcohol aqueous solution of the silane coupling agent, the weight ratio of the silane coupling agent, the alcohol and the water is 1:2-4:0.1-0.3;
[0023] Preferably, the curing temperature is 80-100° C. and the curing time is 0.5-2 h.
[0024] Preferably, in step S3, the heat pressing curing is performed at a pressure of 2-5 MPa, a temperature of 200-260° C., and a time of 1-2 h.
[0025] In the present invention, the mobile phone cover includes a ceramic substrate, an adhesive layer and a basalt fiber reinforced CPI resin layer. Since the basalt fiber reinforced CPI resin has high strength and good toughness, it can improve the overall strength and toughness of the mobile phone cover, and can also achieve lightness and thinness; at the same time, the basalt fiber reinforced CPI resin layer and the ceramic substrate are connected by the adhesive layer, which can greatly improve the connection firmness between the basalt fiber reinforced CPI resin layer and the ceramic matrix, and avoid the phenomenon of falling off. DETAILED DESCRIPTION
[0026] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0027] Example 1
[0028] A basalt fiber reinforced CPI resin mobile phone cover, the preparation method of which comprises the following steps:
[0029] (1) processing zirconia ceramic into a sheet with a thickness of 0.3 mm to obtain a ceramic substrate;
[0030] (2) mixing silane coupling agent KH-560, anhydrous ethanol and water in a weight ratio of 1:3:0.2, stirring at room temperature for 1 hour, and then dropping dilute hydrochloric acid to adjust the pH to 4.5 to obtain an alcohol aqueous solution of the silane coupling agent; coating the alcohol aqueous solution of the silane coupling agent on a ceramic substrate, baking at 90° C. for 1 hour to form a binder layer with a thickness of 30 μm, and obtaining a ceramic substrate with a binder layer;
[0031] (3) Basalt fiber cloth (plain weave, diameter 13 μm, surface density 300 g / m 2 , thickness 0.15mm) was added to a 1wt% hexadecyltrimethylammonium bromide aqueous solution and soaked, taken out and dried to obtain a pretreated basalt fiber cloth; 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether was added to N-methylpyrrolidone and dissolved completely, and then an equal molar amount of 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride and 1wt% of triethylamine of 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether were added under nitrogen protection, and the reaction was stirred at room temperature for 3h to obtain a CPI resin glue with a solid content of 35wt%; the CPI resin glue was coated on both sides of the pretreated basalt fiber cloth, heated to 180°C at a heating rate of 10°C / min, and then cured for 1h, and the coating amount of the resin glue was 300g / m 2 , obtaining a basalt fiber cloth pre-impregnated with CPI resin glue;
[0032] (4) Two layers of basalt fiber cloth pre-impregnated with CPI resin glue are pasted on a ceramic substrate with an adhesive layer, and hot-pressed at a temperature of 230° C. and a pressure of 3 MPa. After maintaining for 1.5 hours, a basalt fiber reinforced CPI resin layer with a thickness of 0.35 mm is formed, and the mobile phone cover is obtained by cutting and shaping.
[0033] Example 2
[0034] A basalt fiber reinforced CPI resin mobile phone cover, the preparation method of which comprises the following steps:
[0035] (1) processing zirconia ceramic into a sheet with a thickness of 0.3 mm to obtain a ceramic substrate;
[0036] (2) mixing silane coupling agent KH-550, anhydrous ethanol and water in a weight ratio of 1:2:0.3, stirring at room temperature for 1 hour, and then adding dilute hydrochloric acid to adjust the pH to 4.5 to obtain an alcohol aqueous solution of the silane coupling agent; coating the alcohol aqueous solution of the silane coupling agent on a ceramic substrate, baking at 100° C. for 0.5 hour to form a binder layer with a thickness of 30 μm, and obtaining a ceramic substrate with a binder layer;
[0037] (3) Basalt fiber cloth (plain weave, diameter 13 μm, surface density 300 g / m 2 , thickness 0.15mm) was added to a 1wt% hexadecyltrimethylammonium bromide aqueous solution and soaked, taken out and dried to obtain a pretreated basalt fiber cloth; 2,2′-bis(trifluoromethyl)-4,4′-diaminobiphenyl was added to N-methylpyrrolidone and dissolved completely, and then an equal molar amount of 4,4′-(hexafluoroisopropylene) diphthalic anhydride and 1wt% of triethylamine of 2,2′-bis(trifluoromethyl)-4,4′-diaminobiphenyl were added under nitrogen protection, and the reaction was stirred at room temperature for 3h to obtain a CPI resin glue with a solid content of 35wt%; the CPI resin glue was coated on both sides of the pretreated basalt fiber cloth, heated to 200°C at a heating rate of 5°C / min, and then cured for 0.5h, and the coating amount of the resin glue was 300g / m 2 , obtaining a basalt fiber cloth pre-impregnated with CPI resin glue;
[0038] (4) Two layers of basalt fiber cloth pre-impregnated with CPI resin glue are pasted on a ceramic substrate with an adhesive layer and hot-pressed at a temperature of 200° C. and a pressure of 5 MPa. After maintaining for 2 hours, a basalt fiber reinforced CPI resin layer with a thickness of 0.34 mm is formed, which is then cut and shaped to obtain the mobile phone cover.
[0039] Example 3
[0040] A basalt fiber reinforced CPI resin mobile phone cover, the preparation method of which comprises the following steps:
[0041] (1) processing zirconia ceramic into a sheet with a thickness of 0.3 mm to obtain a ceramic substrate;
[0042] (2) mixing silane coupling agent KH-580, anhydrous ethanol and water in a weight ratio of 1:4:0.1, stirring at room temperature for 1 hour, and then dropping dilute hydrochloric acid to adjust the pH to 4.5 to obtain an alcohol aqueous solution of the silane coupling agent; coating the alcohol aqueous solution of the silane coupling agent on a ceramic substrate, baking at 80° C. for 2 hours to form a binder layer with a thickness of 30 μm, and obtaining a ceramic substrate with a binder layer;
[0043] (3) Basalt fiber cloth (plain weave, diameter 13 μm, surface density 300 g / m 2 , thickness 0.15mm) was added to a 1wt% hexadecyltrimethylammonium bromide aqueous solution and soaked, taken out and dried to obtain a pretreated basalt fiber cloth; tetrafluoro-m-phenylenediamine was added to N-methylpyrrolidone and dissolved completely, and then an equimolar amount of pyromellitic anhydride and triethylamine (1wt% of the mass of tetrafluoro-m-phenylenediamine) were added under nitrogen protection, and stirred for reaction at room temperature for 3h to obtain a CPI resin glue with a solid content of 35wt%; the CPI resin glue was coated on both sides of the pretreated basalt fiber cloth, heated to 160°C at a heating rate of 10°C / min, and then cured for 0.5h, and the coating amount of the resin glue was 300g / m 2 , obtaining a basalt fiber cloth pre-impregnated with CPI resin glue;
[0044] (4) Two layers of basalt fiber cloth pre-impregnated with CPI resin glue are pasted on a ceramic substrate with an adhesive layer, and hot-pressed at a temperature of 260° C. and a pressure of 2 MPa. After maintaining for 1 hour, a basalt fiber reinforced CPI resin layer with a thickness of 0.36 mm is formed, and the mobile phone cover is obtained by cutting and shaping.
[0045] Comparative Example 1
[0046] A basalt fiber reinforced CPI resin mobile phone cover, the preparation method of which comprises the following steps:
[0047] (1) processing zirconia ceramic into a sheet with a thickness of 0.3 mm to obtain a ceramic substrate;
[0048] (2) Basalt fiber cloth (plain weave, diameter 13 μm, surface density 300 g / m 2, thickness 0.15mm) was added to a 1wt% hexadecyltrimethylammonium bromide aqueous solution and soaked, taken out and dried to obtain a pretreated basalt fiber cloth; 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether was added to N-methylpyrrolidone and dissolved completely, and then an equal molar amount of 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride and 1wt% of triethylamine of 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether were added under nitrogen protection, and the reaction was stirred at room temperature for 3h to obtain a CPI resin glue with a solid content of 35wt%; the CPI resin glue was coated on both sides of the pretreated basalt fiber cloth, heated to 180°C at a heating rate of 10°C / min, and then cured for 1h, and the coating amount of the resin glue was 300g / m 2 , obtaining a basalt fiber cloth pre-impregnated with CPI resin glue;
[0049] (3) Two layers of basalt fiber cloth pre-impregnated with CPI resin glue are pasted on the ceramic substrate and hot-pressed at a temperature of 230° C. and a pressure of 3 MPa. After maintaining for 1.5 hours, a basalt fiber reinforced CPI resin layer with a thickness of 0.35 mm is formed, which is then cut and shaped to obtain the mobile phone cover.
[0050] Comparative Example 2
[0051] A basalt fiber reinforced CPI resin mobile phone cover, the preparation method of which comprises the following steps:
[0052] (1) processing zirconia ceramic into a sheet with a thickness of 0.3 mm to obtain a ceramic substrate;
[0053] (2) mixing silane coupling agent KH-560, anhydrous ethanol and water in a weight ratio of 1:3:0.2, stirring at room temperature for 1 hour, and then dropping dilute hydrochloric acid to adjust the pH to 4.5 to obtain an alcohol aqueous solution of the silane coupling agent; coating the alcohol aqueous solution of the silane coupling agent on a ceramic substrate, baking at 90° C. for 1 hour to form a binder layer with a thickness of 30 μm, and obtaining a ceramic substrate with a binder layer;
[0054] (3) Basalt fiber cloth (plain weave, diameter 13 μm, surface density 300 g / m 2, thickness 0.15mm) was added to a 1wt% hexadecyltrimethylammonium bromide aqueous solution and soaked, taken out and dried to obtain a pretreated basalt fiber cloth; 4,4′-diaminodiphenyl ether was added to N-methylpyrrolidone and dissolved completely, and then an equal mole of pyromellitic anhydride and triethylamine (1wt% of 4,4′-diaminodiphenyl ether) were added under nitrogen protection, and stirred for reaction at room temperature for 3h to obtain a CPI resin glue with a solid content of 35wt%; the CPI resin glue was coated on both sides of the pretreated basalt fiber cloth, heated to 180°C at a heating rate of 10°C / min, and then cured for 1h. The coating amount of the resin glue was 300g / m 2 , obtaining a basalt fiber cloth pre-impregnated with CPI resin glue;
[0055] (4) Two layers of basalt fiber cloth pre-impregnated with CPI resin glue are pasted on a ceramic substrate with an adhesive layer, and hot-pressed at a temperature of 230° C. and a pressure of 3 MPa. After maintaining for 1.5 hours, a basalt fiber reinforced CPI resin layer with a thickness of 0.35 mm is formed, and the mobile phone cover is obtained by cutting and shaping.
[0056] Comparative Example 3
[0057] A basalt fiber reinforced CPI resin mobile phone cover, the preparation method of which comprises the following steps:
[0058] (1) processing zirconia ceramic into a sheet with a thickness of 0.3 mm to obtain a ceramic substrate;
[0059] (2) mixing silane coupling agent KH-560, anhydrous ethanol and water in a weight ratio of 1:3:0.2, stirring at room temperature for 1 hour, and then dropping dilute hydrochloric acid to adjust the pH to 4.5 to obtain an alcohol aqueous solution of the silane coupling agent; coating the alcohol aqueous solution of the silane coupling agent on a ceramic substrate, baking at 90° C. for 1 hour to form a binder layer with a thickness of 30 μm, and obtaining a ceramic substrate with a binder layer;
[0060] (3) 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether was added to N-methylpyrrolidone and dissolved completely. Then, under nitrogen protection, 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride and triethylamine (1 wt% of the mass of 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether) were added in equal moles. After stirring and reacting for 3 hours at room temperature, a CPI resin adhesive having a solid content of 35 wt% was obtained. The CPI resin adhesive was coated on a basalt fiber cloth (plain weave, diameter 13 μm, surface density 300 g / m 2 , thickness 0.15mm) on both sides, heated to 180℃ at a heating rate of 10℃ / min and then cured for 1h. The coating amount of the resin glue is 300g / m 2, obtaining a basalt fiber cloth pre-impregnated with CPI resin glue;
[0061] (4) Two layers of basalt fiber cloth pre-impregnated with CPI resin glue are pasted on a ceramic substrate with an adhesive layer, and hot-pressed at a temperature of 230° C. and a pressure of 3 MPa. After maintaining for 1.5 hours, a basalt fiber reinforced CPI resin layer with a thickness of 0.35 mm is formed, and the mobile phone cover is obtained by cutting and shaping.
[0062] Weight reduction ratio test: Weigh the mass of the mobile phone cover plate described in the embodiment and the comparative example and the pure ceramic zirconia ceramic substrate of the same size and thickness of 0.68 mm respectively, and calculate the weight reduction ratio of the mobile phone cover plate described in the embodiment and the comparative example relative to the pure ceramic zirconia ceramic substrate of the same size and thickness of 0.68 mm;
[0063] Impact resistance test: a 30g steel ball was freely dropped from a height of 20cm to impact the mobile phone cover plates of the embodiment and the comparative example, once at each height, rising 5cm each time, until cracks appeared on the ceramic surface;
[0064] Temperature and humidity resistance test: The mobile phone cover plates described in the embodiment and the comparative example were placed in an environment with a temperature of 75° C. and a humidity of 95% for 168 hours, and the interface of the mobile phone cover plate was observed to see if there was any peeling phenomenon.
[0065] The results are shown in Table 1 below.
[0066] Table 1 Performance test results of the mobile phone cover plates of the embodiments and comparative examples
[0067]
[0068] As can be seen from the above table, the mobile phone cover according to the embodiment of the present invention has improved impact performance to varying degrees compared with the comparative example, and the fiber-reinforced resin layer and the ceramic matrix have a better connection firmness.
[0069] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A mobile phone cover plate of basalt fiber reinforced CPI resin, characterized in that: It includes a ceramic substrate, a bonding agent layer and a basalt fiber reinforced CPI resin layer.
2. According to claim 1, the basalt fiber reinforced CPI resin mobile phone cover is characterized in that: The adhesive layer is formed by coating an alcohol aqueous solution of a silane coupling agent on a ceramic substrate and then solidifying the solution; Preferably, the silane coupling agent is at least one of KH-550, KH-560, KH-570 or KH-580.
3. The mobile phone cover of basalt fiber reinforced CPI resin according to claim 1 or 2, characterized in that: The basalt fiber reinforced CPI resin layer is formed by hot pressing and curing a basalt fiber cloth pre-impregnated with CPI resin glue.
4. The mobile phone cover of basalt fiber reinforced CPI resin according to claim 3, characterized in that: The CPI resin glue is a fluorinated polyimide resin glue; Preferably, the fluorinated polyimide resin glue is obtained by copolymerizing a fluorinated diamine monomer and a non-fluorinated dianhydride monomer or a fluorinated dianhydride monomer in an organic solvent; Preferably, the fluorine-containing diamine monomer is at least one of 2,2′-bis(trifluoromethyl)-4,4′-diaminophenyl ether, 2,2′-bis(trifluoromethyl)-4,4′-diaminobiphenyl, 2,2-bis-(3-amino-4-hydroxyphenyl)hexafluoropropane or tetrafluoro-metaphenylenediamine; the dianhydride monomer is at least one of 4,4′-(hexafluoroisopropylene)diphthalic anhydride, 1,2,4,5-cyclohexanetetracarboxylic anhydride, 1,2,3,4-cyclobutanetetracarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic anhydride or pyromellitic anhydride.
5. The basalt fiber reinforced CPI resin mobile phone cover according to claim 4, characterized in that: The basalt fiber cloth is also immersed in an aqueous solution containing hexadecyltrimethylammonium bromide before being pre-impregnated with the CPI resin glue.
6. The mobile phone cover of basalt fiber reinforced CPI resin according to any one of claims 1 to 5, characterized in that: The ceramic substrate is at least one of a zirconium oxide ceramic substrate, an aluminum oxide ceramic substrate or a silicon carbide ceramic substrate.
7. The mobile phone cover of basalt fiber reinforced CPI resin according to any one of claims 1 to 6, characterized in that: The thickness of the ceramic substrate is 0.1-1 mm, the thickness of the adhesive layer is 5-50 μm, and the thickness of the fiber-reinforced resin layer is 0.1-1 mm.
8. A method for preparing a mobile phone cover plate of basalt fiber reinforced CPI resin according to any one of claims 1 to 7, characterized in that: The steps include: S1. providing a ceramic substrate; S2, coating the ceramic substrate with an alcohol aqueous solution of a silane coupling agent, and forming a binder layer after curing; S3, pasting basalt fiber cloth pre-impregnated with CPI resin glue on the adhesive layer, and forming a basalt fiber reinforced CPI resin layer after hot pressing and curing to obtain the mobile phone cover.
9. The method for preparing the mobile phone cover of basalt fiber reinforced CPI resin according to claim 8, characterized in that: In step S2, in the alcohol aqueous solution of the silane coupling agent, the weight ratio of the silane coupling agent, the alcohol and the water is 1:2-4:0.1-0.3; Preferably, the curing temperature is 80-100° C. and the curing time is 0.5-2 h.
10. The method for preparing the mobile phone cover of basalt fiber reinforced CPI resin according to claim 8 or 9, characterized in that: In step S3, the heat pressing curing is performed under a pressure of 2-5 MPa, a temperature of 200-260° C., and a time of 1-2 h.
Citation Information
Patent Citations
Treatment method for modifying titanium boride ceramic surface by using silane coupling agent
CN105622166A
Basalt fiber composite material and preparation method thereof
CN108752929A
Shell assembly, manufacturing method thereof and electronic equipment
CN113199825A
Basalt fiber silica gel coating cloth and preparation method thereof