Activated aluminum oxide for purifying high-density polyethylene and preparation method of activated aluminum oxide
By preparing activated alumina with high content of ultra-large pores and micropores, the problem of inappropriate pore size distribution in the prior art is solved, and its ability to adsorb catalyst impurities is significantly improved, and the quality of polyethylene products is improved.
Patent Information
- Application Number
- CN202410975515.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-06
AI Technical Summary
The pore size distribution of existing activated alumina is not suitable, and it is difficult to effectively adsorb the remaining catalyst impurities in the Ziegler-Natta polymerization reaction, affecting the quality of polyethylene products.
By mixing aluminum hydroxide raw materials with additives, crushing, flash roasting, pore formation, accumulation and granulation, hydration reaction and activation roasting, activated alumina with high content of ultra-large pores and micropores, controlling roasting and hydration Reaction conditions to improve pore structure.
The content of super-large pores and micropores in activated alumina is significantly improved, its ability to adsorb catalyst impurities is enhanced, and the quality of polyethylene products is improved.
Smart Images

Figure CN119080041A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of fine alumina materials, and in particular to an activated alumina for purifying high-density polyethylene and a preparation method thereof. Background Art
[0002] In the Ziegler-Natta polymerization reaction, VOCl3 is generally used as an initiator and TiCl4 is used as a catalyst to carry out ethylene polymerization to prepare polyethylene. After the reaction is completed, TiCl4 and VOCl3 will remain in the polyethylene working solution, which will eventually cause the plastic products to turn yellow, thus seriously affecting the quality of the plastic products. Therefore, it is generally necessary to add a purifier to the working solution after the Ziegler-Natta polymerization reaction to absorb the catalyst impurities such as TiCl4 and VOCl3 remaining in the polyethylene working solution to improve the quality of polyethylene products. At present, the special adsorbent for the Ziegler-Natta polymerization reaction is a high-density polyethylene (HDPE) purifier.
[0003] The active alumina component plays a decisive role in the HDPE purifier, and the pore structure of the active alumina determines the purification effect of the HDPE purifier. However, the pore size of the active alumina is generally concentrated, and the content of macropores above 75nm and micropores below 2.4nm is insufficient, making it difficult to effectively adsorb catalyst impurities in the Ziegler-Natta polymerization reaction. Summary of the invention
[0004] The present application provides an activated alumina for purification of high-density polyethylene and a preparation method thereof, in order to solve the following technical problem: how to increase the content of super macropores and micropores in the activated alumina.
[0005] In a first aspect, the present application provides a method for preparing activated alumina for purification of high-density polyethylene, the preparation method comprising:
[0006] Mixing the aluminum hydroxide raw material and the additive to obtain a mixed material;
[0007] Crushing the mixed material to obtain aluminum hydroxide powder with a preset particle size;
[0008] Flash roasting the aluminum hydroxide powder having a preset particle size to obtain a p-alumina raw material;
[0009] The pore-forming agent and the ρ-alumina raw material are mixed, and then stacked and granulated to obtain a molded product with a preset bulk density;
[0010] The molded product is subjected to a hydration reaction, and then activated and calcined to obtain activated alumina;
[0011] Wherein, the additive is the activated alumina;
[0012] The initial temperature of the flash roasting is 955°C to 965°C, and the terminal temperature of the flash roasting is 395°C to 405°C;
[0013] The peak temperature of the hydration reaction is ≤90°C, and the time of the hydration reaction is ≤24h;
[0014] The activation calcination temperature is greater than 240°C.
[0015] Optionally, the weight ratio of the additive to the aluminum hydroxide raw material is 5% to 10%.
[0016] Optionally, taking the raw material flow direction as the positive direction, the temperature gradient of the flash roasting is 90° C. / m to 100° C. / m.
[0017] Optionally, the preset particle size is 10.0 μm to 12.5 μm.
[0018] Optionally, the pore-forming agent comprises an alkaline solution, and the content of alkaline solute in the alkaline solution is 4.5% to 10%.
[0019] Optionally, the initial bulk density of the stacking granulation is 1.00 g / mL to 1.08 g / mL, and the preset bulk density is 0.70 g / mL to 0.78 g / mL.
[0020] Optionally, the hydration reaction time is 10 h to 24 h.
[0021] Optionally, the peak temperature of the activation roasting is 270° C. to 300° C., and the time of the activation roasting is ≥1.5 h; taking the raw material flow direction as the positive direction, the temperature gradient of the activation roasting is ≤20° C. / m.
[0022] In a second aspect, the present application provides an activated alumina for purification of high-density polyethylene, wherein the activated alumina is obtained by the preparation method described in the first aspect, and the activated alumina is pseudo-boehmite.
[0023] Optionally, the content of microporous activated alumina in the activated alumina is ≥10%, and the content of ultra-macroporous activated alumina in the activated alumina is ≥15%; wherein the microporous activated alumina is an activated alumina with a pore diameter of less than 2.4 nm, and the ultra-macroporous activated alumina is an activated alumina with a pore diameter of more than 75 nm.
[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0025] The embodiment of the present application provides a preparation method of activated alumina for purification of high-density polyethylene, the preparation method comprising: mixing an aluminum hydroxide raw material and an additive to obtain a mixture; crushing the mixture to obtain an aluminum hydroxide powder with a preset particle size; flash roasting the aluminum hydroxide powder with a preset particle size to obtain a ρ-alumina raw material; mixing a pore-forming agent and the ρ-alumina raw material, and then stacking and granulating to obtain a molded product with a preset bulk density; hydrating the molded product, and then performing activation roasting to obtain activated alumina; wherein the additive is the activated alumina; the initial temperature of the flash roasting is 955°C to 965°C, and the terminal temperature of the flash roasting is 395°C to 405°C; the peak temperature of the hydration reaction is ≤90°C, and the time of the hydration reaction is ≤24h; the temperature of the activation roasting is >240°C. The additive may be activated alumina, which may be used to replace part of the aluminum hydroxide raw material. In the subsequent hydration reaction, the activated alumina will not undergo hydration reaction again. On the other hand, the activated alumina that has undergone hydration reaction in the subsequent hydration reaction stage may be blocked between the ρ-alumina raw materials to reduce the intensity of the reaction of the ρ-alumina raw materials during the hydration reaction, thereby avoiding the concentrated dispersion of a large amount of ρ-alumina raw materials, thereby increasing the content of ultra-large-pore activated alumina in the activated alumina. In addition, the initial temperature of the flash calcination may be 955°C to 965°C, and the terminal temperature of the flash calcination may be 395°C to 405°C, which may The specific surface area of the ρ-alumina raw material and the crystalline phase purity of the ρ-alumina raw material after the hydration reaction are controlled to ultimately increase the content of super-large pores and micro-pores of the activated alumina; in addition, the peak temperature of the hydration reaction can be ≤90°C, and the hydration reaction time can be ≤24h, so as to control the progress of the hydration reaction of the molded product, thereby ultimately increasing the content of super-large pore activated alumina; in addition, the temperature of the activation calcination can be >240°C, so as to promote the molded product after the hydration reaction to be transformed into an activated alumina product with good specific surface area, pore volume and pore size distribution through activation calcination, thereby ultimately increasing the content of super-large pores and micro-pore activated alumina. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A schematic flow chart of a method for preparing activated alumina for high-density polyethylene purification provided in an embodiment of the present application;
[0029] Figure 2 A schematic diagram of an activated alumina for purification of high-density polyethylene provided in an embodiment of the present application;
[0030] Figure 3 This is a schematic diagram of the characterization results of activated alumina for purification of high-density polyethylene provided in Example 1 of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0033] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0034] Figure 1 The schematic diagram of the process for preparing a method for high-density polyethylene purification using activated alumina provided in an embodiment of the present application is shown by way of example;
[0035] like Figure 1 As shown, the present application embodiment provides a method for preparing activated alumina for purification of high-density polyethylene, the preparation method comprising:
[0036] S1. mixing the aluminum hydroxide raw material and the additive to obtain a mixture;
[0037] S2. crushing the mixture to obtain aluminum hydroxide powder having a preset particle size;
[0038] S3. The aluminum hydroxide powder having a preset particle size is flash calcined to obtain a ρ-alumina raw material;
[0039] S4. The pore-forming agent and the ρ-alumina raw material are mixed, and then stacked and granulated to obtain a molded product having a preset bulk density;
[0040] S5. The molded product is subjected to a hydration reaction, followed by activation calcination to obtain activated alumina;
[0041] Wherein, the additive is the activated alumina;
[0042] The initial temperature of the flash roasting is 955°C to 965°C, and the terminal temperature of the flash roasting is 395°C to 405°C;
[0043] The peak temperature of the hydration reaction is ≤90°C, and the time of the hydration reaction is ≤24h;
[0044] The activation calcination temperature is greater than 240°C;
[0045] The initial temperature of the flash roasting may be 955°C, 956°C, 957°C, 958°C, 959°C, 960°C, 961°C, 962°C, 963°C, 964°C or 965°C.
[0046] The endpoint temperature of the flash roasting can be 395°C, 396°C, 397°C, 398°C, 399°C, 400°C, 401°C, 402°C, 403°C, 404°C or 405°C.
[0047] It should be noted that the pore former and the ρ-alumina raw material can be mixed by spraying the pore former.
[0048] In some optional embodiments, the weight ratio of the additive to the aluminum hydroxide raw material is 5% to 10%;
[0049] In these embodiments, the weight ratio of the additive to the aluminum hydroxide raw material can be 5% to 10%, which can ensure that the mixture has a sufficient amount of the additive. Since the activated alumina as an additive has already undergone a hydration reaction, during the hydration reaction stage of the subsequent molded product, the additive will be blocked between the particles of the ρ-alumina raw material to reduce the intensity of the reaction of the ρ-alumina raw material during the hydration reaction, thereby avoiding the concentrated dispersion of a large amount of ρ-alumina raw material, thereby increasing the content of ultra-large pore activated alumina in the activated alumina.
[0050] The weight ratio of the additive to the aluminum hydroxide raw material can be 5%, 6%, 7%, 8%, 9% or 10%.
[0051] In some optional embodiments, taking the raw material flow direction as the positive direction, the temperature gradient of the flash calcination is 90° C. / m to 100° C. / m.
[0052] In these embodiments, with the raw material flow direction as the positive direction, the temperature gradient of the flash roasting can be 90°C / m to 100°C / m, and the temperature distribution of the flash roasting can be controlled, thereby controlling the specific surface area of the ρ-alumina raw material and the crystalline phase purity of the ρ-alumina raw material after the hydration reaction, so as to ultimately increase the content of super large pores and micropores of the activated alumina.
[0053] The temperature gradient of the flash calcination may be 90°C / m, 91°C / m, 92°C / m, 93°C / m, 94°C / m, 95°C / m, 96°C / m, 97°C / m, 98°C / m, 99°C / m or 100°C / m.
[0054] In some optional embodiments, the preset particle size is 10.0 μm to 12.5 μm;
[0055] In these embodiments, the preset particle size can be 10.0 μm to 12.5 μm, which can ensure that the aluminum hydroxide powder has sufficient specific surface area and particle size to obtain a ρ-alumina raw material with an appropriate pore structure, thereby facilitating the subsequent hydration reaction and ultimately increasing the content of ultra-large pores and micropores in the activated alumina.
[0056] The preset particle size may be 10.0 μm, 10.5 μm, 11.0 μm, 11.5 μm, 12.0 μm or 12.5 μm.
[0057] In some optional embodiments, the pore-forming agent comprises an alkaline solution, and the content of alkaline solute in the alkaline solution is 4.5% to 10%.
[0058] In these embodiments, the pore-forming agent may include an alkaline solution, and the content of the alkaline solute in the alkaline solution may be 4.5% to 10%. The alkaline solute may be used to provide a sufficient amount of alkaline substance for the activated alumina, and the sufficient amount of alkaline substance may decompose the ρ-alumina raw material to increase the specific surface area and pore structure of the ρ-alumina raw material, thereby increasing the content of ultra-large pore activated alumina in the activated alumina; in addition, the alkaline solute may use sodium bicarbonate, and sodium bicarbonate is an environmentally friendly additive that can avoid the pollution of the environment by the alkaline solute.
[0059] The content of alkaline solute in the alkaline solution can be 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5% or 10.0%.
[0060] In some optional embodiments, the initial bulk density of the stacked granulation is 1.00 g / mL to 1.08 g / mL, and the preset bulk density is 0.70 g / mL to 0.78 g / mL.
[0061] In these embodiments, the initial bulk density of the stacked granulation can be 1.00 g / mL to 1.08 g / mL, and the preset bulk density can be 0.70 g / mL to 0.78 g / mL, which can promote sufficient mixing between the ρ-alumina raw material and the pore-forming agent to improve the pore density and stacking of the molded product, thereby increasing the content of ultra-large pores and micropores of the activated alumina during the subsequent hydration reaction.
[0062] The initial bulk density of the stacked granulation may be 1.00 g / mL, 1.01 g / mL, 1.02 g / mL, 1.03 g / mL, 1.04 g / mL, 1.05 g / mL, 1.06 g / mL, 1.07 g / mL, or 1.08 g / mL.
[0063] The preset bulk density may be 0.70 g / m3, 0.71 g / m3, 0.72 g / m3, 0.73 g / m3, 0.74 g / m3, 0.75 g / m3, 0.76 g / m3, 0.77 g / m3 or 0.78 g / m3.
[0064] In some optional embodiments, the hydration reaction time is 10 h to 24 h.
[0065] In these embodiments, the hydration reaction time can be 10 hours to 24 hours, which can prompt the hydration reaction to last for a sufficient time. The hydration reaction of sufficient time can prompt the molded product to have a sufficient specific surface area and a sufficient pore structure, so as to ultimately increase the content of ultra-large pores and micropores of the activated alumina.
[0066] The hydration reaction time can be 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h.
[0067] In some optional embodiments, the peak temperature of the activation roasting is 270°C to 300°C, the time of the activation roasting is ≥1.5h; taking the raw material flow direction as the positive direction, the temperature gradient of the activation roasting is ≤20°C / m.
[0068] In these embodiments, the peak temperature of the activation roasting can be 270°C to 300°C, and the activation roasting time can be >1.5h; and the temperature gradient of the activation roasting can be ≤20°C / m with the raw material flow direction as the positive direction, which can promote the activation roasting to proceed fully, so as to promote the separation of the pore-forming agent and the activated alumina product, thereby forming a sufficient amount of pore structure in the activated alumina, so as to ultimately increase the content of ultra-large pores and micropores in the activated alumina.
[0069] The peak temperature of the activation roasting may be 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, or 300°C.
[0070] Figure 2 A schematic diagram of an activated alumina for purification of high-density polyethylene provided in an embodiment of the present application is exemplarily shown;
[0071] Based on a general inventive concept, such as Figure 2As shown, an embodiment of the present application provides an activated alumina for purification of high-density polyethylene, wherein the activated alumina is obtained by the preparation method, and the activated alumina is pseudo-boehmite.
[0072] The activated alumina is realized based on the above-mentioned preparation method. The specific steps of the preparation method can refer to the above-mentioned embodiment. Since the activated alumina adopts part or all of the technical solutions of the above-mentioned embodiment, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be described one by one here.
[0073] In some optional embodiments, the content of microporous activated alumina in the activated alumina is ≥10%, and the content of ultra-macroporous activated alumina in the activated alumina is ≥15%; wherein the microporous activated alumina is an activated alumina with a pore diameter of less than 2.4 nm, and the ultra-macroporous activated alumina is an activated alumina with a pore diameter of more than 75 nm;
[0074] In these embodiments, the content of microporous activated alumina in the activated alumina can be ≥10%, and the content of ultra-macroporous activated alumina in the activated alumina can be ≥15%, which can enable the activated alumina to have sufficient ultra-macroporous activated alumina and microporous activated alumina, thereby effectively adsorbing catalyst impurities in the Ziegler-Natta polymerization reaction.
[0075] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.
[0076] Example 1
[0077] like Figure 1 As shown, a method for preparing activated alumina for purifying high-density polyethylene comprises:
[0078] S1. mixing the aluminum hydroxide raw material and the additive to obtain a mixture;
[0079] S2. crushing the mixture to obtain aluminum hydroxide powder having a preset particle size;
[0080] S3. Flash calcining the aluminum hydroxide powder at a preset temperature to obtain a ρ-alumina raw material;
[0081] S4. The pore-forming agent and ρ-alumina raw material are mixed in and out, and then stacked and granulated to obtain a molded product having a preset bulk density;
[0082] S5. The molded product is subjected to a hydration reaction, and then activated and calcined to obtain activated alumina;
[0083] Wherein, the additive is activated alumina;
[0084] The initial temperature of flash roasting was 955°C, and the terminal temperature of flash roasting was 395°C;
[0085] The peak temperature of the hydration reaction was 85 °C, and the hydration reaction time was 24 h;
[0086] The weight ratio of the additive to the aluminum hydroxide raw material is 10%.
[0087] Taking the raw material flow direction as the positive direction, the temperature gradient of flash roasting is 100°C / m.
[0088] The preset particle size is 10.0 μm.
[0089] The pore-forming agent comprises an alkaline solution, the content of the alkaline solute in the alkaline solution is 10%, and the alkaline solute is sodium bicarbonate.
[0090] The initial bulk density of the stacked granulation was 1.08 g / mL and the bulk volume was 0.5 m 3 The particle size of the molded product is 1.6mm~2.8mm; the preset bulk density is 0.78g / mL.
[0091] The peak temperature of the activation calcination is 300°C, and the activation calcination time is 1.5h.
[0092] Example 2
[0093] Based on the contents disclosed in Example 1, the following modifications are further made:
[0094] The initial temperature of flash roasting is 960°C, and the terminal temperature of flash roasting is 400°C;
[0095] The peak temperature of the hydration reaction was 90 °C, and the hydration reaction time was 24 h;
[0096] The weight ratio of the additive to the aluminum hydroxide raw material is 5%.
[0097] Taking the raw material flow direction as the positive direction, the temperature gradient of flash roasting is 90°C / m.
[0098] The preset particle size is 10.5 μm.
[0099] The content of alkaline solute in the alkaline solution is 4.5%.
[0100] The initial bulk density of the stacked granulation was 1.00 g / mL and the bulk volume was 0.3 m 3 , the preset bulk density is 0.71g / mL.
[0101] The peak temperature of the activation calcination is 290°C, and the activation calcination time is 2.0 h.
[0102] Example 3
[0103] Based on the contents disclosed in Example 1, the following modifications are further made:
[0104] The initial temperature of flash roasting was 965°C, and the terminal temperature of flash roasting was 405°C;
[0105] The peak temperature of the hydration reaction was 88 °C, and the hydration reaction time was 16 h;
[0106] The weight ratio of the additive to the aluminum hydroxide raw material is 7%.
[0107] Taking the raw material flow direction as the positive direction, the temperature gradient of flash roasting is 95°C / m.
[0108] The preset particle size is 11.5 μm.
[0109] The content of alkaline solute in the alkaline solution is 8%.
[0110] The initial bulk density of the stacked granules was 1.04 g / mL and the bulk volume was 0.4 m 3 , the preset bulk density is 0.74g / mL.
[0111] The peak temperature of the activation calcination is 270°C, and the activation calcination time is 3.0 h.
[0112] Example 4
[0113] Based on the contents disclosed in Example 1, the following modifications are further made:
[0114] The initial temperature of flash roasting was 960°C, and the terminal temperature of flash roasting was 398°C;
[0115] The peak temperature of the hydration reaction was 82 °C, and the hydration reaction time was 15 h;
[0116] The weight ratio of the additive to the aluminum hydroxide raw material is 8%.
[0117] Taking the raw material flow direction as the positive direction, the temperature gradient of flash roasting is 97°C / m.
[0118] The preset particle size is 12.0 μm.
[0119] The content of alkaline solute in the alkaline solution is 6%.
[0120] The initial bulk density of the stacked granulation was 1.05 g / mL and the bulk volume was 0.45 m 3 , the preset bulk density is 0.73g / mL.
[0121] The peak temperature of the activation roasting is 278°C, and the activation roasting time is 2.1h.
[0122] Example 5
[0123] Based on the contents disclosed in Example 1, the following modifications are further made:
[0124] The initial temperature of flash roasting was 955°C, and the terminal temperature of flash roasting was 402°C;
[0125] The peak temperature of the hydration reaction was 85 °C, and the hydration reaction time was 18 h;
[0126] The weight ratio of the additive to the aluminum hydroxide raw material is 5%.
[0127] Taking the raw material flow direction as the positive direction, the temperature gradient of flash roasting is 105℃ / m.
[0128] The preset particle size is 10.5 μm.
[0129] The content of alkaline solute in the alkaline solution is 7%.
[0130] The initial bulk density of the stacked granulation was 1.02 g / mL and the bulk volume was 0.35 m 3 , the preset bulk density is 0.72g / mL.
[0131] The peak temperature of the activation roasting is 295°C, and the activation roasting time is 1.6h.
[0132] Example 6
[0133] Based on the contents disclosed in Example 1, the following modifications are further made:
[0134] The initial temperature of flash roasting was 958°C, and the terminal temperature of flash roasting was 397°C;
[0135] The peak temperature of the hydration reaction was 85 °C, and the hydration reaction time was 17 h;
[0136] The weight ratio of the additive to the aluminum hydroxide raw material is 6.5%.
[0137] Taking the raw material flow direction as the positive direction, the temperature gradient of flash roasting is 99°C / m.
[0138] The preset particle size is 12.2 μm.
[0139] The content of alkaline solute in the alkaline solution is 7%.
[0140] The initial bulk density of the stacked granulation was 1.03 g / mL and the bulk volume was 0.50 m 3 , the preset bulk density is 0.73g / mL.
[0141] The peak temperature of the activation roasting is 270°C, and the activation roasting time is 2.5h.
[0142] Related experiments and effect data:
[0143] 1. The pore diameter of the activated alumina product obtained in Example 1 was tested. The results are as follows: Figure 3 The results show that the content of super-large pore activated alumina with a pore diameter of more than 75nm in the activated alumina product is ≥15%, and the content of micro-pore activated alumina with a pore diameter of less than 2.4nm is ≥10%.
[0144] 2. The activated alumina products obtained in Examples 1 to 6 were statistically analyzed, and their specific parameters were statistically analyzed. The results are shown in Table 1.
[0145] Table 1 Parameters of activated alumina products obtained in various embodiments
[0146]
[0147] In Table 1, the specific surface area was measured in accordance with ISO9277 international standard.
[0148] Loss on ignition, Na2O content, bulk density, abrasion, particle size and strength are tested according to the standard of Q / CHINALCO / ZLGF A003-2022.
[0149] In addition, the content of ultra-large pore activated alumina with a pore diameter of more than 75 nm and the content of micro-pore activated alumina with a pore diameter of less than 2.4 nm in the activated alumina products obtained in various embodiments and comparative examples were statistically analyzed, and the results are shown in Table 2.
[0150] Table 2 Particle size distribution of activated alumina products obtained in various examples and comparative examples
[0151]
[0152] As can be seen from Table 2, the preparation method of activated alumina for high-density polyethylene purification provided in the embodiment of the present application uses activated alumina to replace part of the aluminum hydroxide raw material to reduce the reaction intensity of the ρ-alumina raw material during the hydration reaction, thereby increasing the content of ultra-large pores and micropores in the activated alumina; in addition, the temperature field of the flash calcination is controlled to control the specific surface area of the ρ-alumina raw material and the crystalline phase purity of the ρ-alumina raw material after the hydration reaction, so as to ultimately increase the content of ultra-large pores and micropores in the activated alumina; in addition, the process conditions of the hydration reaction are controlled to ultimately increase the content of ultra-large pores and micropores in the activated alumina; in addition, the temperature of the activation calcination combines the characteristics of the activated alumina and the decomposition temperature of sodium bicarbonate to ultimately increase the content of ultra-large pores and micropores of the activated alumina.
[0153] In addition, an activated alumina for purifying high-density polyethylene provided in an embodiment of the present application has a content of super-large-pore activated alumina with a pore diameter of more than 75 nm ≥ 15%, and a content of micro-pore activated alumina with a pore diameter of less than 2.4 nm ≥ 10%, which is beneficial for adsorbing catalyst impurities such as TiCl4 and VOCl3 in the polyethylene working fluid in the Ziegler-Natta polymerization reaction, so as to achieve the purpose of purifying the polyethylene working fluid and improving the quality of plastic products.
[0154] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.
Claims
1. A method for preparing activated alumina for high-density polyethylene purification, characterized in that: The preparation method comprises: mixing the aluminum hydroxide raw material and the additive to obtain a mixture; Crushing the mixed material to obtain aluminum hydroxide powder with a preset particle size; flash calcining the aluminum hydroxide powder having a predetermined particle size to obtain a p-alumina raw material; The pore-forming agent and the ρ-alumina raw material are mixed, and then stacked and granulated to obtain a molded product with a preset bulk density; performing a hydration reaction on the molded product, and then performing activation roasting to obtain activated alumina; Wherein, the additive is the activated alumina; The initial temperature of the flash roasting is 955°C to 965°C, and the terminal temperature of the flash roasting is 395°C to 405°C; The peak temperature of the hydration reaction is ≤90°C, and the time of the hydration reaction is ≤24h; The activation calcination temperature is greater than 240°C.
2. The preparation method according to claim 1, characterized in that The weight ratio of the additive to the aluminum hydroxide raw material is 5% to 10%.
3. The preparation method according to claim 1, characterized in that Taking the raw material flow direction as the positive direction, the temperature gradient of the flash roasting is 90° C. / m to 100° C. / m.
4. The preparation method according to claim 1, characterized in that The preset particle size is 10.0 μm to 12.5 μm.
5. The preparation method according to claim 1, characterized in that The pore-forming agent comprises an alkaline solution, and the content of alkaline solute in the alkaline solution is 4.5% to 10%.
6. The preparation method according to claim 1, characterized in that The initial bulk density of the stacked granulation is 1.00 g / mL to 1.08 g / mL, and the preset bulk density is 0.70 g / mL to 0.78 g / mL.
7. The preparation method according to claim 1, characterized in that The hydration reaction time is 10h to 24h.
8. The preparation method according to claim 1, characterized in that The peak temperature of the activation roasting is 270° C. to 300° C., the activation roasting time is ≥1.5 h; with the raw material flow direction as the positive direction, the temperature gradient of the activation roasting is ≤20° C. / m.
9. An activated alumina for purification of high-density polyethylene, characterized in that: The activated alumina is obtained by the preparation method according to any one of claims 1 to 8, and the activated alumina is pseudo-boehmite.
10. The activated alumina according to claim 9, characterized in that The content of microporous activated alumina in the activated alumina is ≥10%, and the content of ultra-macroporous activated alumina in the activated alumina is ≥15%; wherein, the microporous activated alumina is activated alumina with a pore diameter of less than 2.4 nm, and the ultra-macroporous activated alumina is activated alumina with a pore diameter of more than 75 nm.
Citation Information
Cited By
Preparation method for alumina aerogel
WO2026124344A1