In2O3 composite TiO2 aerogel hydrogen-sensitive material and preparation method thereof

Through In2O3 composite TiO2 aerogel material, the existing TiO2 aerogel hydrogen sensor has been solved, and the rapid response and high stability detection of hydrogen is achieved, and the modern industry's demand for hydrogen detection is met. .

CN119080052APending Publication Date: 2024-12-06YANGTZE DELTA REGION INST (QUZHOU) UNIV OF ELECTRONIC SCI & TECH OF CHINA
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410577281.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing TiO2 aerogel hydrogen sensors have problems such as poor stability, long response time and poor gas selectivity, which cannot meet the needs of modern industry for hydrogen detection.

Method used

Using In2O3 composite TiO2 aerogel material, block TiO2 aerogel is prepared and composited with In2O3, and porous three-dimensional structure In2O3/TiO2 aerogel is synthesized by hydrothermal method to prepare a gas sensor.

Benefits of technology

It achieves a fast response and recovery time to 100ppm H2, with high linearity and good stability, and has excellent performance for multiple cycle detection of 200ppm H2, with a 13.4-fold increase in response value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080052A_ABST
    Figure CN119080052A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of an In2O3 composite TiO2 aerogel hydrogen-sensitive material. The preparation method comprises the following steps: step 1, preparing blocky TiO2 aerogel; step 2, preparation of an In2O3 / TiO2 compound precursor: weighing InCl3, deionized water, a hydrochloric acid solution and ammonia water, and uniformly mixing and stirring; adding the blocky TiO2 aerogel obtained in the step 1 into a mixed solution for soaking; carrying out hydrothermal reaction on the mixed solution soaked with the blocky TiO2 aerogel, then cooling a product to room temperature, washing and drying to obtain compound precursor powder; the In2O3 / TiO2 composite aerogel synthesized by a hydrothermal method has a porous three-dimensional structure, the maximum response of the composite aerogel sensor to 100 ppmH2 at the optimal working temperature is more than 17, and the composite aerogel sensor has quick response and recovery time and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen-sensitive sensing materials, and specifically relates to an In2O3 composite TiO2 aerogel hydrogen-sensitive material and a preparation method thereof. Background Art

[0002] Hydrogen (H2) is an energy storage carrier. In addition to its high energy density and easy production, it produces water when burning air or discharging in fuel cells, which is green and pollution-free. Therefore, hydrogen energy has long been considered a promising alternative to fossil fuel energy. Because H2 molecules are small and chemically active, the widespread use of H2 is accompanied by the risk of H2 leakage and explosion. Therefore, there are safety hazards that cannot be ignored during the storage, transportation and application of H2. Therefore, in order to prevent H2 leakage, it is necessary to develop a reliable and relatively cheap H2 gas sensor to detect hydrogen.

[0003] Among many gas sensors, the most typical one is the resistive hydrogen sensor synthesized from n-type semiconductor metal oxide (SMO) materials such as TiO2, SnO2, and ZnO. Its response principle is that the oxygen in the air is physically adsorbed or chemically adsorbed to form oxygen ions attached to the SMO surface, thereby forming SMO defects and capturing electrons from the SMO conduction band, thereby forming an electron depletion layer, increasing the ground state resistance of the sensor. Subsequently, H2 undergoes an oxidation-reduction reaction with the oxygen species on the surface to generate free electrons, which reduces the resistance of the SMO material and achieves the detection purpose.

[0004] Among them, TiO2 is an n-type semiconductor material with a wide band gap (3.2eV), which is non-toxic and abundant, and has good chemical stability and biocompatibility. It is widely used in photocatalytic hydrogen production, photocatalytic reduction, lithium batteries, gas sensing and other fields.

[0005] Although TiO2 metal semiconductor sensors have been widely studied, due to material structural factors such as low specific surface area, existing TiO2 raw sensors generally have shortcomings such as narrow H2 detection range, low response, and poor gas selectivity, which are not enough for actual H2 detection. TiO2 aerogel has the characteristics of light weight and high porosity, and is a nanomaterial with high specific surface area. This porous structure is conducive to gas diffusion and meets the three-dimensional structure requirements of gas-sensitive materials. However, the current aerogel hydrogen sensors have poor stability, long response time and recovery time, which cannot meet the needs of modern industry. Summary of the invention

[0006] In order to overcome the technical defects of the prior art, the present invention discloses an In2O3 composite TiO2 aerogel hydrogen-sensitive material and a preparation method thereof.

[0007] The method for preparing the In2O3 composite TiO2 aerogel hydrogen-sensitive material of the present invention comprises the following steps:

[0008] Step 1. Prepare bulk TiO2 aerogel;

[0009] Step 2. Preparation of In2O3 / TiO2 composite precursor:

[0010] Weigh InCl3, deionized water, hydrochloric acid solution and ammonia water and mix them evenly;

[0011] Take the block TiO2 aerogel obtained in step 1 and add it into the mixed solution for soaking;

[0012] The ratio of InCl3, deionized water, hydrochloric acid solution, ammonia water and block TiO2 aerogel is 0.01g-1g: 30-50ml: 0.1ml-0.5ml: 10ml-15ml: 0.7g-1g;

[0013] The concentrations of hydrochloric acid and ammonia water are 0.01-0.1 mol / L and 10-15 mol / L respectively;

[0014] The mixed solution soaked with the block TiO2 aerogel is subjected to a hydrothermal reaction, and then the product is cooled to room temperature, and the obtained white precipitate is collected, washed and dried to obtain a composite precursor powder.

[0015] Step 3. Preparation of In2O3 / TiO2 composite:

[0016] The composite precursor powder obtained in step 2 is calcined at 400° C.-800° C. in an air atmosphere for 8 h-10 h, and after natural cooling, the In2O3 composite TiO2 aerogel hydrogen-sensitive material is collected.

[0017] Preferably, the step 1 is specifically:

[0018] Weigh anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate, put them into a beaker and stir them to mix them evenly to form solution A; wherein the volume ratio of anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate is 2:0.05-0.1:1;

[0019] Weigh anhydrous ethanol, anhydrous acetic acid, deionized water, and DMF, put them into a beaker and stir to mix them evenly to form solution B; wherein the volume ratio of anhydrous ethanol, anhydrous acetic acid, deionized water, and DMF is 10:2.5:3:1;

[0020] Solution B was added to solution A and stirred at a volume ratio of 1:1. After stirring evenly, the obtained gel precursor solution was placed in a thermostat at 30°C-60°C to obtain a wet gel;

[0021] The wet gel was subjected to solvent exchange aging and then dried to obtain block TiO2 aerogel.

[0022] Preferably, the solvent exchange aging is specifically: soaking the wet gel with ethanol, changing it every 6-10 hours, and continuing for more than 4 times.

[0023] Preferably, in step 2, the ratio of InCl3 to bulk TiO2 aerogel is 7-7.5:1.

[0024] An In2O3 composite TiO2 aerogel hydrogen-sensitive material is obtained by using the preparation method as described above.

[0025] The present invention synthesizes TiO2 aerogel by a sol-gel method, and further synthesizes In2O3 / TiO2 composite aerogel by a hydrothermal method; the composite aerogel material has a porous three-dimensional structure, and when used as a gas sensor, the prepared composite aerogel sensor has a maximum response of 17.48096 to 100ppmH2 at an optimal working temperature. The In2O3 / TiO2 composite aerogel structure prepared by the present invention has a fast response and recovery time, high linearity, and good stability to multiple cycles of 200ppmH2. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A comparison diagram of the dynamic response curves of 100ppm H2 at different concentrations of the In2O3 / TiO2 composite material prepared by the present invention;

[0027] Figure 2 A comparison of the 100ppm H2 dynamic response curves of the In2O3 / TiO2 composite material prepared by the present invention at different concentrations and that of single TiO2;

[0028] Figure 3 A schematic diagram of the dynamic response test curve of the sensor prepared using 15wt% In2O3 / TiO2 composite material to 100-1000ppm H2;

[0029] Figure 4 Schematic diagram of repeated test curves of 200 ppm H2 for a sensor prepared using 15 wt% In2O3 / TiO2 composite material. DETAILED DESCRIPTION

[0030] The following is combined with Figures 1 to 3 , the specific implementation modes of the present invention are further described in detail.

[0031] The method for preparing the In2O3 composite TiO2 aerogel hydrogen-sensitive material of the present invention comprises the following steps:

[0032] Weigh anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate (Ti(OC4H9)4) and put them into a beaker and stir to mix them evenly to form solution A; wherein the volume ratio of anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate is 2:0.05-0.1:1;

[0033] Weigh anhydrous ethanol, anhydrous acetic acid, deionized water, and DMF (anhydrous N,N-dimethylformamide) and put them into a beaker and stir to mix them evenly to form solution B; wherein the volume ratio of anhydrous ethanol, anhydrous acetic acid, deionized water, and DMF is 10:2.5:3:1;

[0034] Add the aqueous solution B to the non-aqueous solution A and stir to react. The volume ratio of the two is 1:1.

[0035] The direct hydrolysis of tetrabutyl titanate and deionized water to obtain titanium oxide is not conducive to the subsequent wet gel formation; the product obtained by pre-dispersing them separately and then mixing them is more uniform. The role of anhydrous acetic acid is as a pH regulator and can also be used as a chelating agent. Anhydrous ethyl acetate is used as a solvent to mix the two reactants evenly and control the hydrolysis rate of tetrabutyl titanate.

[0036] After being stirred evenly, the obtained gel precursor solution is transferred to a thermostat and allowed to stand in a thermostat at 30° C. to 60° C. for 12 h to 24 h to obtain a wet gel.

[0037] The wet gel was soaked in ethanol for solvent exchange and aging, and the solvent was changed every 8 hours for 6 times. It was then placed in a supercritical drying device for drying to obtain a block-like white TiO2 aerogel.

[0038] The purpose of using ethanol to soak the wet gel for solvent exchange and aging is to wash and remove the remaining water and other organic impurities in the wet gel.

[0039] In step 1, the blocky white TiO2 aerogel can be used to further prepare TiO2 aerogel powder: the dried TiO2 aerogel white powder is placed in a porcelain boat, the porcelain boat is placed in a tubular furnace, and calcined at 400°C-800°C in an air atmosphere for 8h-10h. After natural cooling, the TiO2 aerogel white powder is collected.

[0040] Step 2. Preparation of In2O3 / TiO2 composite precursor: Weigh InCl3, deionized water, hydrochloric acid solution and ammonia water into a beaker and stir to mix them evenly. Take the blocky white TiO2 aerogel in step 1 and soak it in the mixed solution. Transfer the mixed solution to a reactor for hydrothermal reaction, then cool the product to room temperature, collect the obtained white precipitate, wash it with deionized water several times, and put it in an oven to dry to obtain a white composite precursor powder.

[0041] The hydrochloric acid provides an acidic environment to prevent the hydrolysis of indium trichloride, and the high concentration of ammonia water can promote the formation of a complex with indium ions. The role of the hydrothermal reaction is to form a cubic crystal structure of In(OH)3, and after calcination, the grain size is uniform, which facilitates the formation of a three-dimensional porous In2O3 structure.

[0042] Step 3. Preparation of In2O3 / TiO2 composite: Weigh the composite precursor powder obtained in step 2 and put it into a porcelain boat, place the porcelain boat in a tube furnace, calcine at 400℃-800℃ in an air atmosphere for 8h-10h, and after natural cooling, collect the In2O3 / TiO2 composite in the form of light yellow powder.

[0043] Further, in step 2, the weighed ratios of InCl3, deionized water, hydrochloric acid solution, ammonia water and block TiO2 aerogel are 0.01g-1g: 30-50ml: 0.1ml-0.5ml: 10ml-15ml: 0.7g-1g;

[0044] By adjusting the mass ratio of InCl3 and bulk TiO2 aerogel, the mass ratios of In2O3 / TiO2 in the white composite precursor powder were 0.5 / 99.5, 5 / 95, 15 / 85, and 30 / 70, respectively.

[0045] The In2O3 / TiO2 composite prepared in step 3 is used in a wide range of hydrogen gas sensing. The specific electrode preparation method is as follows:

[0046] 5 mg of the prepared In2O3 / TiO2 composite was ground with ethanol to form a uniform paste. The resulting slurry was then applied to the surface of the interdigital electrode (i.e., Au-coated alumina electrode) to form a thin layer. In order to improve the stability of the sensing layer, the interdigital electrode sheet was annealed at 300°C in air atmosphere for 2 hours. Specific embodiment 1:

[0048] Preparation of TiO2 precursor: Weigh anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate (Ti(OC4H9)4) into a beaker and stir for 20 minutes to mix them evenly to form solution A.

[0049] Weigh anhydrous ethanol, anhydrous acetic acid, deionized water, and anhydrous N,N-dimethylformamide (DMF), put them into a beaker and stir for 20 minutes to mix them evenly to form solution B.

[0050] The aqueous solution B was added to the non-aqueous solution A and stirred, and the gel precursor solution was transferred to a thermostat at 30°C for 24 hours to achieve wet gelation. The wet gel was soaked in ethanol for solvent exchange and aging, and the solvent was replaced every 8 hours for 6 times, and then dried in a supercritical drying device to obtain blocky white TiO2 aerogel.

[0051] Embodiment 2:

[0052] Preparation of TiO2: Weigh the pre-dried TiO2 aerogel white powder and put it into a porcelain boat. Place the porcelain boat in a tubular furnace and calcine it at 400°C in an air atmosphere for 10 hours. After natural cooling, collect the TiO2 aerogel white powder.

[0053] Embodiment 3:

[0054] Preparation of In2O3 / TiO2 composite precursor: InCl3, deionized water, hydrochloric acid solution and ammonia water were weighed and stirred in a beaker. The concentrations of hydrochloric acid and ammonia water were 0.01 mol / L and 13 mol / L respectively. The mixture was uniformly mixed to obtain a mixed solution. The blocky white TiO2 aerogel obtained in Example 1 was added to the mixed solution. The mixed solution was transferred to a reactor for hydrothermal reaction, and then the product was cooled to room temperature. The obtained white precipitate was collected, washed with deionized water for several times, and dried in an oven to obtain a white powder.

[0055] Embodiment 4:

[0056] Preparation of In2O3 / TiO2 composite: The white powder obtained in Example 3 was weighed and put into a porcelain boat, which was placed in a muffle furnace and calcined at 400°C in an air atmosphere for 10 hours. After natural cooling, the pale yellow powder of the In2O3 / TiO2 composite was collected. The obtained powders were divided into 4 groups, namely 0.5wt% In2O3 / TiO2, 5wt% In2O3 / TiO2, 15wt% In2O3 / TiO2, and 30wt% In2O3 / TiO2.

[0057] The test method for hydrogen gas sensing performance in this embodiment is as follows:

[0058] Take 5 mg of the prepared light yellow powder and grind it with ethanol to form a uniform paste. Then apply the obtained slurry on the surface of the interdigital electrode (i.e., Au-coated alumina electrode) to form a thin layer. In order to improve the stability of the sensing layer, the interdigital electrode sheet is annealed in an air atmosphere at 300°C for 2 hours. The test gas H2 is in a high-purity steel cylinder, and the ratio is 5000ppm H2 standard gas, which contains 0.5% H2, 99.5% N2, and high-purity air in a standard steel cylinder. The H2 standard gas is mixed with air by setting a program to control the dynamic gas distribution platform to obtain a H2 gas with a concentration of 100ppm-1000ppm. First, high-purity air is introduced until the resistance value of the test electrode is stabilized to Ra, and then a target gas (mixed H2) of a specific concentration is introduced until the resistance value drops to a stable value to obtain Rg. The response value is Ra / Rg. The larger the ratio, the greater the decrease in the resistance value of the electrode in hydrogen. The hydrogen sensing performance was measured in a dual-channel tester with dynamic gas flow, and the single TiO2 phase and 0.5wt% In2O3 / TiO2, 5wt% In2O3 / TiO2, 15wt% In2O3 / TiO2, 30wt% In2O3 / TiO2 composites were measured at the optimal working temperature (single TiO2 is 475℃, 0.5wt% In2O3 / TiO2 is 450℃, 5wt% In2O3 / TiO2 is 450℃, 15wt% In2O3 / TiO2 is 450℃, 30wt% In2O3 / TiO2 is 450℃) to 100ppm H2 dynamic response curve, 100-1000ppm H2 dynamic response, dynamic response-recovery curve and its cyclic response test to 200ppm were tested. The response value, response / recovery time and stability of the sample were analyzed by the response-recovery curve.

[0059] from Figure 1 and Figure 2 It can be seen that after the introduction of H2, the response value (Ra / Rg) of the In2O3 / TiO2-based sensor increases and the resistance decreases. After the introduction of air, the resistance increases, indicating that its response to hydrogen is still an n-type response, and the compounding of In2O3 does not change the chemical properties of TiO2 aerogel. Figure 1 and Figure 2 It can be seen that 15wt% In2O3 doping is the best compounding amount. Compared with the pure sample, it improves the response to H2, and the sensitivity reaches more than 17. At 100ppm, the response value increases by 13.4 times. Its high response is due to the porous structure characteristics of the aerogel, the nn heterojunction effect and the oxygen vacancies. The large amount of chemically adsorbed oxygen on the surface greatly increases the resistance of the sensor in the air. The ratio of InCl3 and bulk TiO2 aerogel in step 2 corresponding to this doping is approximately 7-7.5:1.

[0060] Figure 3 The 15wt% In2O3 / TiO2 dynamic response test of 100-1000ppm H2. It can be seen from the dynamic response-recovery characteristic curve to H2 that the 15wt% In2O3 / TiO2 sample has a good dynamic response to H2, and the 100-1000ppmH response test results of the 15wt% In2O3 / TiO2 composite show that the sample has good linearity.

[0061] Figure 4 This is a repeatability test of the 15wt% In2O3 / TiO2 composite to 200ppm H2. The response curve shows that the 15wt% In2O3 / TiO2 sample has good repeatability.

[0062] The foregoing describes various preferred embodiments of the present invention. Unless the preferred implementation modes in various preferred embodiments are obviously self-contradictory or based on a certain preferred implementation mode, various preferred implementation modes can be arbitrarily superimposed and used in combination. The embodiments and specific parameters in the embodiments are only for clearly describing the invention verification process of the inventor, and are not used to limit the patent protection scope of the present invention. The patent protection scope of the present invention shall still be based on its claims. All equivalent structural changes made using the contents of the description and drawings of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an In2O3 composite TiO2 aerogel hydrogen-sensitive material, characterized in that: The steps include: Step 1. Prepare bulk TiO2 aerogel; Step 2. Preparation of In2O3 / TiO2 composite precursor: Weigh InCl3, deionized water, hydrochloric acid solution and ammonia water and mix them evenly; Take the block TiO2 aerogel obtained in step 1 and add it into the mixed solution for soaking; The ratio of InCl3, deionized water, hydrochloric acid solution, ammonia water and block TiO2 aerogel is 0.01g-1g: 30-50ml: 0.1ml-0.5ml: 10ml-15ml: 0.7g-1g; The concentrations of hydrochloric acid and ammonia water are 0.01-0.1 mol / L and 10-15 mol / L respectively; The mixed solution soaked with the block TiO2 aerogel is subjected to a hydrothermal reaction, and then the product is cooled to room temperature, and the obtained white precipitate is collected, washed and dried to obtain a composite precursor powder. Step 3. Preparation of In2O3 / TiO2 composite: The composite precursor powder obtained in step 2 is calcined at 400° C.-800° C. in an air atmosphere for 8 h-10 h, and after natural cooling, the In2O3 composite TiO2 aerogel hydrogen-sensitive material is collected.

2. The method for preparing the In2O3 composite TiO2 aerogel hydrogen-sensitive material according to claim 1, characterized in that: The step 1 is specifically as follows: Weigh anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate, put them into a beaker and stir them to mix them evenly to form solution A; wherein the volume ratio of anhydrous ethanol, anhydrous acetic acid, and tetrabutyl titanate is 2:0.05-0.1:1; Weigh anhydrous ethanol, anhydrous acetic acid, deionized water, and DMF, put them into a beaker and stir to mix them evenly to form solution B; wherein the volume ratio of anhydrous ethanol, anhydrous acetic acid, deionized water, and DMF is 10:2.5:3:1; Solution B was added to solution A and stirred at a volume ratio of 1:

1. After stirring evenly, the obtained gel precursor solution was placed in a thermostat at 30°C-60°C to obtain a wet gel; The wet gel was subjected to solvent exchange aging and then dried to obtain block TiO2 aerogel.

3. The method for preparing the In2O3 composite TiO2 aerogel hydrogen-sensitive material according to claim 2, characterized in that: The solvent exchange aging is specifically as follows: soaking the wet gel in ethanol, changing the solvent every 6-10 hours, and continuing for more than 4 times.

4. The method for preparing the In2O3 composite TiO2 aerogel hydrogen-sensitive material according to claim 1, characterized in that: In step 2, the ratio of InCl3 to bulk TiO2 aerogel is 7-7.5:

1.

5. An In2O3 composite TiO2 aerogel hydrogen-sensitive material, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 4.

Citation Information

Cited By

  • Pt and Pd co-doped In2O3 / TiO2 resistance type hydrogen sensor

    CN119827585A