Preparation method of superfine cobaltosic oxide
By using cobalt salt, complexing agent and regulator in the preparation of tricobalt oxide, the reaction method of cobalt salt, complexing agent and alkali solution, the problems of insufficient particle size and production complexity in the prior art are solved, and ultrafine with an average particle size below 1.5 μm is achieved Cobalt tetroxide is prepared, with a more uniform and regular product morphology and suitable for industrial production.
Patent Information
- Application Number
- CN202411195153.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-29
AI Technical Summary
It is difficult to prepare ultrafine cobalt tetroxide with a particle size of less than 2μm in the prior art, and in industrial production, the reaction pH and reactant flow rate need to be strictly controlled, which cannot meet the needs of high capacity development of lithium cobalt oxide materials.
By mixing the cobalt salt, complexing agent and regulator with water, and then calcining it with alkali solution, using 1,2 diaminocyclohexanitetaacetic acid and hydrogen peroxide as complexing agent and regulator, control The stirring rate and temperature were used to obtain ultrafine cobalt tetroxide with uniform particle size.
The preparation of ultrafine cobalt tetroxide with an average particle size of less than 1.5μm was achieved, the reaction conditions were easily met, the product morphology was more uniform and regular, and it was suitable for industrial production.
Smart Images

Figure CN119080075A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field, and in particular to a method for preparing ultrafine cobalt tetroxide. Background Art
[0002] The transition metal oxide cobalt tetroxide is widely used as a precursor for lithium cobalt oxide cathode materials. With the rapid development of electronic products and the need for higher and more stable energy storage, the requirements for cobalt tetroxide are getting higher and higher. It is well known that the morphology of cobalt tetroxide has a significant effect on its physical and electrochemical properties. The blending of cobalt tetroxide with large and small particles can increase the compaction density to increase the energy density of lithium cobalt oxide materials. The market's requirements for small particle size will become smaller and smaller.
[0003] At present, medium and large particles of cobalt tetroxide are relatively mature in the market, but ultrafine cobalt tetroxide (<2μm) has not yet been industrialized. In order to meet the development direction of high capacity of lithium cobalt oxide materials, a mature preparation method of ultrafine cobalt tetroxide is particularly important. For example, CN112850803A discloses a method for synthesizing highly tapped ultrafine cobalt tetroxide, in which a cobalt salt solution and an alkaline solution are added to a base liquid containing a complexing agent, and the flow rate of the cobalt salt solution and the alkaline solution is controlled and the pH value is maintained between 10.5-11.5 for stirring and reacting to obtain a cobalt salt precipitate, which is then calcined to obtain cobalt tetroxide. This method can obtain particles with a size concentration of 1.5-2.5μm and a tap density of 2.1-2.6g / cm 3 However, this method requires strict control of the pH and flow rate of the reaction, which brings difficulties to industrial production and cannot produce cobalt tetroxide with finer particle size.
[0004] There is still a need to provide an effective method for the problems existing in the preparation of ultrafine cobalt tetroxide. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a method for preparing ultrafine cobalt tetroxide, comprising: The cobalt salt, the complexing agent, the regulator and water are mixed to prepare a cobalt-containing solution; The cobalt-containing solution is mixed with an alkaline solution for reaction, and the insoluble matter is collected and calcined to obtain ultrafine cobalt trioxide.
[0006] It should be noted that the type of cobalt salt in the present invention does not need to be strictly limited. For example, it can be at least one of cobalt chloride hexahydrate, cobalt sulfate heptahydrate, cobalt nitrate hexahydrate, and cobalt acetate tetrahydrate.
[0007] Furthermore, the complexing agent is at least one of 1,2-diaminocyclohexanetetraacetic acid, ethylenediaminetetraacetic acid, nitrilotriacetic acid, and 5-sulfosalicylic acid.
[0008] Furthermore, the regulator is hydrogen peroxide with a mass concentration of 27.5%-35%.
[0009] Furthermore, the amounts of cobalt salt, complexing agent and regulator in the cobalt-containing solution are 100-140 g / L, 1-5 g / L and 60-80 mL / L respectively.
[0010] Furthermore, the calcination is first heated to 400-500°C at a rate of 3-10°C / min and kept warm for 3-8h; then heated to 650-750°C at a rate of 3-10°C / min and kept warm for 3-8h.
[0011] Furthermore, when the cobalt-containing solution and the sodium hydroxide solution are mixed and reacted, the cobalt-containing solution is added to the alkaline solution at a volume ratio of 1:3-10 at a stirring rate of 400-600 rpm.
[0012] Furthermore, the flow rate of adding the cobalt-containing solution is 20-50 L / h, and the reaction is continued for 10-30 minutes after the addition of the cobalt-containing solution is completed.
[0013] Furthermore, the concentration of the alkaline solution is 0.5-1 mol / L.
[0014] The present invention also provides ultrafine cobalt tetroxide, which is obtained by the above-mentioned preparation method.
[0015] The present invention also provides the use of the ultrafine cobalt tetroxide in the preparation of lithium cobalt oxide.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The raw materials of the present invention are cheap and easy to obtain, and there is no need to add a special complexing agent and strictly control the feeding rate of the cobalt-containing solution and the precipitant solution. The ultrafine cobalt tetraoxide with uniform particle size and an average particle size of less than 1.5 μm can be obtained through the combined action of the complexing agent and the regulator. Overall, compared with the ultrafine cobalt tetraoxide currently prepared by the hydrothermal synthesis-calcination method, the present invention has the advantages of easy reaction conditions and more uniform and regular product morphology, and has a good prospect for application in industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 The scanning electron microscope image of the ultrafine cobalt oxide prepared in Example 1 is shown; Figure 2 The scanning electron microscope image of the ultrafine cobalt oxide prepared in Example 2 is shown; Figure 3 The scanning electron microscope image of the ultrafine cobalt oxide prepared in Comparative Example 1 is shown; Figure 4 The scanning electron microscope image of the ultrafine cobalt oxide prepared in Comparative Example 2 is shown; Figure 5 The scanning electron microscope image of the ultrafine cobalt trioxide prepared in Comparative Example 3 is shown. DETAILED DESCRIPTION
[0019] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0020] The following will be combined with the specific embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] It should be noted that, since there is already 10 mol / L sodium hydroxide in the examples, it is used as the mother solution and diluted to the required concentration when used.
[0022] Example 1 A method for preparing ultrafine cobalt trioxide, comprising the following steps: S1. Dissolve 600 g of cobalt chloride hexahydrate in 5 L of water under stirring, then add 10 g of 1,2-diaminocyclohexanetetraacetic acid and stir evenly, then add 350 mL of hydrogen peroxide (mass fraction 30%) and stir evenly to obtain a cobalt-containing solution; S2, adding 25L of water to a 50L reactor, then setting the speed to 600rpm to start stirring and adding 1.6L of 10mol / L sodium hydroxide mother solution, and then passing 5L of the cobalt-containing solution prepared in step S1 at a flow rate of 30L / h. After the addition of the cobalt-containing solution, continue stirring and reacting for 20min; after the reaction is completed, filter press, wash, and dry to obtain a precursor; S3, heating the precursor prepared in step S2 to 450°C at a rate of 5°C / min and keeping the temperature for 6 hours; then heating it to 700°C at a rate of 5°C / min and keeping the temperature for 6 hours; passing the calcined product through a 400-mesh sieve to obtain ultrafine cobalt oxide powder.
[0023] Example 2 A method for preparing ultrafine cobalt trioxide, comprising the following steps: S1. Dissolve 600 g of cobalt chloride hexahydrate in 5 L of water under stirring, then add 10 g of 1,2-diaminocyclohexanetetraacetic acid and stir evenly, then add 350 mL of hydrogen peroxide (mass fraction 30%) and stir evenly to obtain a cobalt-containing solution; S2, adding 25L of water to a 50L reactor, then setting the speed to 600rpm to start stirring and adding 1.6L of 10mol / L sodium hydroxide mother solution, and then passing 5L of the cobalt-containing solution prepared in step S1 at a flow rate of 30L / h. After the addition of the cobalt-containing solution, continue stirring and reacting for 20min; after the reaction is completed, filter press, wash, and dry to obtain a precursor; S3, heating the precursor prepared in step S2 to 450°C at a rate of 5°C / min and keeping the temperature for 6 hours; then heating it to 700°C at a rate of 5°C / min and keeping the temperature for 6 hours; passing the calcined product through a 400-mesh sieve to obtain ultrafine cobalt oxide powder.
[0024] Comparative Example 1 A method for preparing ultrafine cobalt trioxide, comprising the following steps: S1. Dissolve 600 g of cobalt chloride hexahydrate in 5 L of water under stirring, then add 10 g of 1,2-diaminocyclohexanetetraacetic acid and stir evenly to obtain a cobalt-containing solution; S2, adding 25L of water to a 50L reactor, then setting the speed to 600rpm to start stirring and adding 1.6L of 10mol / L sodium hydroxide mother solution, and then passing 5L of the cobalt-containing solution prepared in step S1 at a flow rate of 30L / h. After the addition of the cobalt-containing solution, continue stirring and reacting for 20min; after the reaction is completed, filter press, wash, and dry to obtain a precursor; S3, heating the precursor prepared in step S2 to 450°C at a rate of 5°C / min and keeping the temperature for 6 hours; then heating it to 700°C at a rate of 5°C / min and keeping the temperature for 6 hours; passing the calcined product through a 400-mesh sieve to obtain ultrafine cobalt oxide powder.
[0025] Comparative Example 2 S1. Dissolve 600 g of cobalt chloride hexahydrate in 5 L of water under stirring, then add 350 mL of hydrogen peroxide (mass fraction 30%) and stir evenly to obtain a cobalt-containing solution; S2, adding 25L of water to a 50L reactor, then setting the speed to 600rpm to start stirring and adding 1.6L of 10mol / L sodium hydroxide mother solution, and then passing 5L of the cobalt-containing solution prepared in step S1 at a flow rate of 30L / h. After the addition of the cobalt-containing solution, continue stirring and reacting for 20min; after the reaction is completed, filter press, wash, and dry to obtain a precursor; S3, heating the precursor prepared in step S2 to 450°C at a rate of 5°C / min and keeping the temperature for 6 hours; then heating it to 700°C at a rate of 5°C / min and keeping the temperature for 6 hours; passing the calcined product through a 400-mesh sieve to obtain ultrafine cobalt oxide powder.
[0026] Comparative Example 3 S1. Dissolve 600 g of cobalt chloride hexahydrate in 5 L of water under stirring, then add 10 g of 1,2-diaminocyclohexanetetraacetic acid and stir evenly, then add 350 mL of hydrogen peroxide (mass fraction 30%) and stir evenly to obtain a cobalt-containing solution; S2, adding 25L of water to a 50L reactor, then setting the speed to 600rpm to start stirring and adding 1.6L of 10mol / L sodium hydroxide mother solution, and then passing 5L of the cobalt-containing solution prepared in step S1 at a flow rate of 30L / h. After the addition of the cobalt-containing solution, continue stirring and reacting for 20min; after the reaction is completed, filter press, wash, and dry to obtain a precursor; S3, heating the precursor prepared in step S2 to 700° C. at a rate of 5° C. / min and keeping the temperature for 12 hours; passing the calcined product through a 400-mesh sieve to obtain ultrafine cobalt trioxide powder.
[0027] Test Case The average particle size of the materials prepared in Examples 1-2 and Comparative Examples 1-3 was tested respectively, and the results are shown in Table 1.
[0028] Table 1 Average particle size results of cobalt oxide materials
[0029] From the test results of Table 1, it can be seen that the embodiments of the present invention have a finer particle size, the median particle size D50 is less than 0.2µm, and the maximum particle size D100 is less than 2µm. In particular, Example 1 has the lowest particle size, and the maximum particle size is less than 1.5µm, which shows that appropriately increasing the concentration of 1,2-diaminocyclohexane tetraacetic acid in the cobalt-containing solution can further reduce the product particle size. However, compared with Example 1, the cobalt-containing solution of Comparative Example 1 does not contain hydrogen peroxide, and the maximum particle size of the prepared cobalt tetroxide is significantly increased, which is almost two orders of magnitude lower than the median particle size D50. This may be because the addition of hydrogen peroxide and 1,2-diaminocyclohexane tetraacetic acid work together to adjust the structure of the cobalt species in the early stage of the reaction, enhance the dispersibility and make it not easy to agglomerate into large particles. Compared with Example 1, the cobalt-containing solution of Comparative Example 2 does not contain 1,2-diaminocyclohexane tetraacetic acid, and the maximum particle size D100 of the prepared cobalt tetroxide is also significantly increased. These results show that the addition of hydrogen peroxide and 1,2-diaminocyclohexane tetraacetic acid can reduce the particle size of cobalt tetroxide. Compared with Example 1, Comparative Example 3 did not adopt the method of calcining at a lower temperature of 450°C and then heating to 700°C for further calcination, but directly calcined at 700°C, and the median particle size D50 and the maximum particle size D100 were also significantly improved.
[0030] The materials prepared in Examples 1-2 and Comparative Examples 1-3 were observed using a scanning electron microscope. The results are as follows: Figure 1-Figure 5 As shown. Combined Figure 1 and Figure 2 It can be seen that the cobalt tetroxide prepared in the embodiment of the present invention has a small particle size and is evenly distributed. Figure 1 and Figure 3 It can be seen that in Comparative Example 1, where the cobalt-containing solution does not contain hydrogen peroxide, the cobalt oxide particles prepared are uneven in size, and there are obviously larger particles. Figure 1 and Figure 4 It can be seen that without adding the complexing agent 1,2-diaminocyclohexane tetraacetic acid, small particles will agglomerate and the particle size distribution of cobalt tetroxide will be uneven. Figure 1 and Figure 5 It can be seen that the direct high-temperature calcination of comparative example 3 will lead to the sintering of small particles of cobalt tetroxide in a cubic structure, with uneven particle distribution and large morphology differences.
[0031] In summary, the raw materials of the present invention are cheap and easy to obtain, and there is no need to add a special complexing agent and strictly control the feed rate of the cobalt-containing solution and the precipitant solution. By adding a regulating agent hydrogen peroxide and a complexing agent 1,2-diaminocyclohexane tetraacetic acid, ultrafine cobalt tetraoxide with uniform particle size and an average particle size of less than 1.5 μm can be obtained. Overall, compared with the ultrafine cobalt tetraoxide currently prepared by hydrothermal synthesis-calcination method, the present invention has the advantages of easy reaction conditions and more uniform and regular product morphology, and has a good prospect for application in industrial production.
[0032] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing ultrafine cobalt trioxide, characterized in that: include, The cobalt salt, the complexing agent, the regulator and water are mixed to prepare a cobalt-containing solution; The cobalt-containing solution is mixed with an alkaline solution for reaction, and the insoluble matter is collected and calcined to obtain ultrafine cobalt trioxide.
2. The method for preparing ultrafine cobalt trioxide according to claim 1, characterized in that: The complexing agent is at least one of 1,2-diaminocyclohexanetetraacetic acid, ethylenediaminetetraacetic acid, nitrilotriacetic acid, and 5-sulfosalicylic acid.
3. The method for preparing ultrafine cobalt trioxide according to claim 1, characterized in that: The regulator is hydrogen peroxide with a mass concentration of 27.5%-35%.
4. The method for preparing ultrafine cobalt tetroxide according to claim 3, characterized in that: The amounts of the cobalt salt, the complexing agent and the regulator in the cobalt-containing solution are 100-140 g / L, 1-5 g / L and 60-80 mL / L respectively.
5. The method for preparing ultrafine cobalt trioxide according to claim 1, characterized in that: The calcination is firstly heated to 400-500°C at a rate of 3-10°C / min and kept at that temperature for 3-8h; then heated to 650-750°C at a rate of 3-10°C / min and kept at that temperature for 3-8h.
6. The method for preparing ultrafine cobalt trioxide according to claim 1, characterized in that: When the cobalt-containing solution and the alkaline solution are mixed for reaction, the cobalt-containing solution is added to the alkaline solution at a volume ratio of 1:3-10 at a stirring rate of 400-600 rpm; The alkaline solution includes at least one of a sodium hydroxide solution or a potassium hydroxide solution.
7. The method for preparing ultrafine cobalt trioxide according to claim 6, characterized in that: The flow rate of adding the cobalt-containing solution is 20-50 L / h, and the reaction is continued for 10-30 minutes after the addition of the cobalt-containing solution is completed.
8. The method for preparing ultrafine cobalt trioxide according to claim 6, characterized in that: The concentration of the alkaline solution is 0.5-1 mol / L.
9. An ultrafine cobalt trioxide, characterized in that: The method is obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the ultrafine cobalt oxide according to claim 9 in the preparation of lithium cobalt oxide.
Citation Information
Patent Citations
Preparation method of cobalt oxide for lithium battery and product prepared by the same
CN101857277A
Method for preparing low-sodium cobaltosic oxide
CN105668650A
Preparation method of ultrafine particle size cobaltosic oxide
CN110255629A
Processes for preparing hydroxides and oxides of various metals and derivatives thereof
CN111867980A
Synthesis method of high-tap-density superfine cobaltosic oxide
CN112850803A