Method for purifying NMMO solvent recovery solution in cellulose fiber prepared by NMMO solvent method
Through multi-stage physical method and anion exchange technology, combined with flocculation and multi-media bed filtration, the problem of impurity removal in NMMO solvent recovery is solved, the recovery rate and equipment life are improved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202411301527.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art cannot effectively remove suspended solids, colored impurities, decomposition products and metal ions during the NMMO solvent recovery process, resulting in low solvent recovery rate, reduced quality of finished fibers, and cumbersome filtration process and inconvenient for industrial scale production.
Multi-stage, deep-level physical filtration combined with anion and cation exchange chemistry method is used to achieve solvents through flocculation treatment, multi-media bed filtration, precision filtration of titanium fibers, anion and cation exchange treatment, combined with turbidity, chromaticity and conductivity detection. Comprehensive purification.
It improves the NMMO solvent recovery rate, simplifies the operating process, extends the service life of the equipment, reduces water and solid waste emissions, and is suitable for industrial scale production.
Smart Images

Figure CN119080311A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solvent recovery and purification, in particular to a method for purifying an NMMO solvent recovery solution in preparing cellulose fibers using an NMMO solvent method. Background Art
[0002] Lyocell fiber is a cellulose fiber prepared by the NMMO solvent method. Its performance is better than that of viscose fiber in all aspects. The product can be naturally degraded and is a good green and environmentally friendly fiber.
[0003] In the production process of solvent-based cellulose fibers, NMMO is a solvent and is very expensive. For the large-scale production of regenerated cellulose fibers, its recycling and reuse is an important step in the solvent-based preparation of cellulose fibers.
[0004] During the production process, the NMMO solvent concentrate is dissolved with cellulose at high temperature, and then after filtration and spinning, it enters the coagulation bath and the aqueous solution of the washing process. The following components should be removed: 1. Suspended solids: mainly part of the dissolved cellulose or cellulose degradation product polysaccharides exist in the solution in the form of agglomerates, which will reduce the efficiency of the evaporator, block the circulation pump, and affect the recovery quality of the solvent; 2. Colored impurities: mainly the decomposition products of NMMO and cellulose at high temperature, and part of them are oxidation products of antioxidant additives. The presence of these substances will reduce the quality of the finished fiber and reduce the recovery rate of NMMO solvent; 3. Decomposition products: here mainly refers to the high-temperature decomposition products of NMMO solvent, namely N-methylmorpholine (NMM) and morpholine (M). Since these products will continue to accumulate in the system, the solubility of the solvent will gradually decrease. At the same time, morpholine will be further oxidized into N-nitrosomorpholine, which is a highly carcinogenic substance and difficult to remove; 4. Metal ions: mainly come from pulp raw materials, as well as metal equipment, pipes, instruments, etc. that come into contact with the cellulose fiber stock solution during the preparation. In particular, iron ions and copper ions will cause the degradation of NMMO solvent and cellulose at high temperatures, and may even cause explosion hazards in severe cases.
[0005] Patent CN1603479A, filed by Donghua University, describes a process for recovering the solvent NMMO. This process involves coarse and fine filtration to remove suspended impurities, using anions and cations to remove metal ions and colored impurities, and then oxidizing the NMMO decomposition products with hydrogen peroxide. However, coarse and fine filtration alone cannot completely remove suspended solids, significantly shortening the useful life of the anions and cations. Furthermore, using hydrogen peroxide to oxidize the decomposition products introduces new impurities, making the process cumbersome.
[0006] Patent CN101089262B applied for by Shanghai Rio Fiber Enterprise Development Co., Ltd. describes the recovery process of solvent NMMO, which includes: solvent recovery to the solvent receiving tank for mixing, then filtering to remove suspended impurities, anion removal of colored impurities, cation removal of metal ions and decomposition products, and colorimetric inspection to determine whether to switch to regeneration. It has the same problem that only one-stage filtration is used to completely remove suspended solids, which will seriously shorten the service life and life of anions and cations. Secondly, after the anion and cation exchange, only one indicator of the solution color value is checked, which cannot reflect the true properties of the solution and the quality of the solution. Summary of the Invention
[0007] To address the above-mentioned issues, the present invention provides a method for purifying NMMO solvent recovery solution from the NMMO solvent process for preparing cellulose fibers. The method comprises stirring and mixing, physical and chemical treatment, and sufficient flocculation, agglomeration, and bridging reactions within a recovery tank. The solution then undergoes multi-stage, in-depth physical filtration, followed by anion and cation exchange chemical removal of remaining impurities. Finally, the solution's colorimeter, turbidity meter, and conductivity are used to comprehensively determine whether the purified solvent's water quality and the need for anion and cation regeneration are necessary. This method simplifies and facilitates the process, facilitates industrial-scale production, and significantly improves the NMMO solvent recovery rate.
[0008] The present invention provides a method for purifying an NMMO solvent recovery solution in preparing cellulose fibers by an NMMO solvent process, the method comprising the following steps:
[0009] adding a flocculant to the NMMO solvent recovery solution to be treated for physicochemical treatment to obtain a first NMMO solvent recovery solution;
[0010] The first NMMO solvent recovery solution is sequentially subjected to solvent coarse filtration, multi-media bed filtration, and solvent fine filtration to obtain a second NMMO solvent recovery solution;
[0011] performing anion exchange treatment on the second NMMO solvent recovery solution to obtain a third NMMO solvent recovery solution;
[0012] The third NMMO solvent recovery solution is subjected to a cation exchange treatment to obtain a purified NMMO solvent recovery solution.
[0013] Furthermore, the method further comprises the following steps:
[0014] The turbidity of the solution after filtration by the multi-media bed filter is detected by a turbidity meter. If the turbidity value is greater than 1 NTU, the multi-media bed filter is started to be regenerated.
[0015] A colorimeter is used to detect the color of the solution after the anion exchange treatment. If the color value is greater than 100 Hazen, the anion resin exchange bed is started for regeneration;
[0016] The conductivity of the solution after the cation exchange treatment is detected by a conductivity meter. If the conductivity is greater than 30 μS / cm, the cation resin exchange bed is started for regeneration.
[0017] Furthermore, the NMMO solvent recovery solution to be processed includes: a dilute foam solvent solution produced in the stock solution workshop of the NMMO solvent method for preparing cellulose fibers, and a coagulation bath solution produced in the spinning workshop of the NMMO solvent method for preparing cellulose fibers;
[0018] In terms of weight percentage, the NMMO concentration in the dilute solvent solution of the foam is 0.6-5%;
[0019] In terms of weight percentage, the NMMO concentration in the coagulation bath solution is 15-25%.
[0020] Furthermore, in terms of weight percentage, the added amount of the flocculant accounts for 0.5-2.5% of the entire material system; the model of the flocculant is FLOPAMFO4650.
[0021] Furthermore, the concentration of the initial diluted solution to which the flocculant is added is 0.1 to 0.5% by weight.
[0022] Furthermore, the solvent coarse filtration adopts an automatic backwashing stacked disc filter, and the working condition parameters of the automatic backwashing stacked disc filter include: using a polypropylene plastic filter plate with an accuracy of 150-250μm, a filtration backwash pressure difference of 0.02-0.05MPa or a set time of 1.5-2.5 hours, and a backwash completion time of 10-30 seconds.
[0023] Furthermore, the filter media of the multi-media bed filter are sequentially filled from top to bottom with pumice with a particle size of 2.5 to 3.5 mm, quartz sand with a particle size of 0.50 to 1.50 mm, and gravel with a particle size of 2.0 to 3.5 mm, and the stacking heights of the filter media layers are 1200 mm, 900 mm, and 300 mm, respectively.
[0024] Furthermore, the solvent fine filtration adopts a titanium fiber precision filter, and the working condition parameters of the titanium fiber precision filter include: the filter element adopts sintered felt, and its filtration accuracy from outside to inside is 3μm, 8μm, 15μm, and 30μm respectively.
[0025] Furthermore, the anion exchange treatment uses an anion fixed bed filled with anion exchange resin, the filling amount of the anion exchange resin in the anion fixed bed is 30-80% of the volume of the exchange bed, and the flow rate of the purified solution containing N-methylmorpholine N-oxide through the exchange bed is 3-6 BV / h; the anion exchange resin is a macroporous, strongly alkaline, epoxy-based anion exchange resin with an -OH group, and the particle size of the epoxy-based anion exchange resin is 20-40 mesh.
[0026] Furthermore, the cationic treatment uses a cationic fixed bed filled with a cationic exchange resin, the filling amount of the cationic exchange resin in the cationic fixed bed is 30-80% of the volume of the exchange bed, the flow rate of the purified solution containing N-methylmorpholine N-oxide through the exchange bed is 3-6 BV / h, the cationic exchange resin is a macroporous, strongly acidic propylene-based cationic exchange resin with a -H group, and the particle size of the propylene-based cationic exchange resin is 20-40 mesh.
[0027] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0028] An embodiment of the present invention provides a method for purifying an NMMO solvent recovery solution in the preparation of cellulose fibers by an NMMO solvent process. The method effectively removes various impurities such as solid particles and metal ions by passing the collected and recovered NMMO solvent aqueous solution through a multi-level, multi-media filter, thereby achieving a process for recovering and purifying the NMMO solvent solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0031] Figure 1 A flow chart of a method for purifying an NMMO solvent recovery solution in preparing cellulose fibers using an NMMO solvent process provided by the present invention;
[0032] Figure 2 Schematic diagram of the process of purifying the NMMO solvent recovery solution in preparing cellulose fibers by the NMMO solvent method according to an embodiment of the present invention. DETAILED DESCRIPTION
[0033] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0035] The present invention provides a method for purifying NMMO solvent recovery solution in preparing cellulose fiber by NMMO solvent method, such as Figure 1 As shown, the method includes the following steps:
[0036] adding a flocculant to the NMMO solvent recovery solution to be treated for physicochemical treatment to obtain a first NMMO solvent recovery solution;
[0037] The first NMMO solvent recovery solution is sequentially subjected to solvent coarse filtration, multi-media bed filtration, and solvent fine filtration to obtain a second NMMO solvent recovery solution;
[0038] performing anion exchange treatment on the second NMMO solvent recovery solution to obtain a third NMMO solvent recovery solution;
[0039] The third NMMO solvent recovery solution is subjected to a cation exchange treatment to obtain a purified NMMO solvent recovery solution.
[0040] An embodiment of the present invention provides a method for purifying an NMMO solvent recovery solution in the preparation of cellulose fibers by an NMMO solvent process. The method effectively removes various impurities such as solid particles and metal ions by passing the collected and recovered NMMO solvent aqueous solution through a multi-level, multi-media filter, thereby achieving a process for recovering and purifying the NMMO solvent solution.
[0041] In some specific embodiments, Figure 2 As shown, the present invention consists of the above six steps, and the solvent recovery solution is filtered step by step at multiple levels to form an organic purification and impurity removal system, which efficiently completes the purification of the NMMO solvent recovery solution; the operation process is simplified and convenient, which greatly promotes the solvent recovery rate of the NMMO solution; the operation and regeneration in the system are all designed with automated processes, without the need for manual operation, thereby improving the automation level of the factory; the system uses reasonable and accurate detection means for the regeneration system to determine whether regeneration has occurred, thereby achieving the purpose of energy saving and environmental protection such as saving water and reducing solid waste emissions, and comprises the following steps:
[0042] The first step is to collect the dilute solvent solution of the foaming glue produced by the raw liquid workshop, the coagulation bath solution produced by the spinning workshop and the flocculant into the solvent water recovery tank for stirring, mixing and physical and chemical treatment;
[0043] The second step is that the solution after physical and chemical treatment is first filtered through an automatic backwashing stacked disc filter to remove most of the solid impurities such as suspended matter and filaments;
[0044] The third step is to pass through a multi-media filter to perform deep filtration to remove the remaining impurities such as agglomerated suspended matter, filaments, and tiny solid particles;
[0045] The fourth step is to further filter the solvent solution after deep filtration through a titanium fiber precision filter to prevent solid particles from contaminating the anion and cation resins;
[0046] The fifth step is to pass the filtrate after fine filtration through an anion exchange bed and a cation exchange bed in sequence to remove all colored groups, metal ions and decomposition products;
[0047] The sixth step is to determine whether the solvent water quality and the cation and cation resin exchange bed are acid-base regenerated by using a turbidity meter, colorimeter or conductivity value.
[0048] Among the above, the first step is NMMO solvent recovery, which adds the foam glue dilute solvent solution, coagulation bath solution and flocculant into the solvent water recovery tank, slowly stirs and fully mixes them, and performs flocculation, agglomeration, bridging and other reactions. The stirrer linear speed is controlled below 6m / s to prevent the stirrer blade linear speed from being too fast, which is not conducive to the agglomeration of particles; the second and third steps are to stir and mix the solution in the solvent water recovery tank, perform physical and chemical treatment, and then filter it through solvent coarse filtration, multi-media bed filter and solvent fine filtration in turn to remove impurities such as agglomerated suspended matter, filaments and tiny solid particles in the solution.
[0049] The filter process design parameters are as follows:
[0050] Solvent coarse filtration: filter accuracy: 150-250μm, operating pressure: 2.5-4.5bar, operating flow rate: 30-80m3 / h (single unit);
[0051] Multi-media bed filtration: Filter media: pumice, quartz sand, gravel; particle sizes: 2.5-3.5mm, 0.5-1.5mm, 2.0-3.5mm; media heights: 1200mm, 900mm, 300mm; design filtration rate: 8-12m / h; water backwash intensity: 8-10L / m 2 .s; Air backwash intensity: 10~15L / m 2 .s; Backwash expansion rate: 50%
[0052] Solvent fine filtration: filter accuracy: 3-30μm, operating pressure: 2.5-4.5bar, operating flow rate: 30-80m3 / h (single unit).
[0053] The filtrate after fine filtration then passes through an anion exchange bed to remove most of the colored groups, metal anions and decomposition products;
[0054] The process design parameters of the anion exchange bed are as follows: filtrate concentration: 10-30% NMMO solution, filtrate temperature: 15-35°C, operating flow rate: 8-12 m / h, exchange resin: type: strong alkaline anion exchange resin with a macroporous structure, particle size: 300-1200 μm, uniformity coefficient: 1.7 (maximum), exchange capacity: 1.15 eq / L, filling height: 2x2000 mm, transition expansion rate: 20% (maximum), backwash expansion rate: 50%. Specifically, commercially available products such as the product model LX-500 of Xi'an Lanxiao Technology New Materials Co., Ltd. can be used.
[0055] The anion exchange solution then passes through a cation exchange bed or a spare cation exchange bed to remove all colored groups, metal cations and decomposition products;
[0056] The process design parameters of the cation exchange bed are as follows: filtrate concentration: 10-30% NMMO solution, filtrate temperature: 15-35°C, operating flow rate: 10-15 m / h; exchange resin: type: strongly acidic cation exchange resin with a macroporous structure, particle size: 300-1200 μm, uniformity coefficient: 1.7 (maximum), exchange capacity: 1.8 eq / L, filling height: 2000 mm, transition expansion rate: 10% (maximum), backwash expansion rate: 100%. Specifically, commercially available products such as the product model LX-150 of Xi'an Lanxiao Technology New Materials Co., Ltd. can be used.
[0057] The turbidity of the solution after filtration through the multi-media bed is detected by a turbidity meter. If the turbidity value is greater than a set value (the initial setting value is 1 NTU), the multi-media bed filter is automatically started for regeneration. The chromaticity of the solution after the anion resin exchange bed is detected by a colorimeter. If the chromaticity value is greater than a set value (the initial setting value is 100 Hazen), the anion resin exchange bed is automatically started for regeneration. The conductivity of the solution after the cation resin exchange bed is detected by a conductivity meter. If the conductivity value is greater than a set value (the initial setting value is 30 μS / cm), the cation resin exchange bed is automatically started for regeneration.
[0058] Among them, the setting value range of the turbidity meter is 0.5~3.5NTU, the setting value range of the colorimeter is 50~150Hazen, and the setting value range of the conductivity meter is 10~150μs / cm.
[0059] The process parameters of the above spare solvent fine filtration, multi-media bed filter and cation-cation resin exchange bed are the same as the above process parameters.
[0060] When the solvent fine filter element is replaced, the multi-media bed filter, and the cation-cation resin exchange bed are automatically regenerated, the online standby equipment is put into operation. The multi-media bed filter is regenerated with desalted water, and the cation-cation resin exchange bed is regenerated with a regeneration solution of 4-6% NaOH aqueous solution and 3-5% HCl aqueous solution for deionization exchange.
[0061] In the present invention, the solvent concentrations are all expressed in mass percentages, and the ratios are all expressed in mass ratios.
[0062] In some specific embodiments, the dilute solvent solution contains NMMO at a concentration of 0.6-5%, and the coagulation bath solution contains NMMO at a concentration of 15-25%.
[0063] In some specific embodiments, the concentration of the flocculant added to the solvent water recovery tank is 0.5-2.5%, and the model of the flocculant is FLOPAMFO4650.
[0064] In some specific embodiments, the concentration of the initial diluted solution to which the flocculant is added is 0.1-0.5%, and the solution is subjected to physicochemical treatment.
[0065] In some specific embodiments, the automatic backwashing stacked disc filter uses a polypropylene plastic filter disc with an accuracy of 150-250 μm, a filtration backwash pressure difference of 0.02-0.05 MPa or a set time of 1.5-2.5 hours, and a backwash completion time of 10-30 seconds.
[0066] In some specific embodiments, the filter media of the multi-media bed filter are filled with pumice, quartz sand and gravel from top to bottom, with particle sizes of 2.5-3.5 mm, 0.50-1.50 mm and 2.0-3.5 mm respectively; the stacking heights of the filter media layers are 1200 mm, 900 mm and 300 mm respectively.
[0067] In some specific embodiments, the filter element of the titanium fiber precision filter adopts sintered felt, and its filtration accuracy from outside to inside is 3μm, 8μm, 15μm, and 30μm respectively.
[0068] In some specific embodiments, the filling amount of the anion exchange resin in the anion fixed bed is 30-80% of the volume of the exchange bed, and the flow rate of the purified solution containing N-methylmorpholine N-oxide through the exchange bed is 3-6 BV / h; the filling amount of the cation exchange resin in the cation fixed bed is 30-80% of the volume of the exchange bed, and the flow rate of the purified solution containing N-methylmorpholine N-oxide through the exchange bed is 3-6 BV / h.
[0069] In some specific embodiments, the anion exchange resin is a macroporous, strongly alkaline, epoxy-based anion exchange resin with an -OH group, and the particle size of the resin is 20 to 40 meshes; the cation exchange resin is a macroporous, strongly acidic, propylene-based cation exchange resin with an -H group, and the particle size of the resin is 20 to 40 meshes.
[0070] In some specific embodiments, the setting value of the turbidity meter is between 0.5 and 3.5 NTU, the setting value of the colorimeter is between 50 and 150 Hazen, and the setting value of the conductivity is between 10 and 150 μS / cm.
[0071] In some specific embodiments, the turbidity meter, colorimeter and conductivity are set so that when any one of the conditions occurs, that is, the turbidity meter value is greater than 1 NTU, the colorimeter value is greater than 100 Hazen, or the conductivity value is greater than 30 μS / cm, the cation and cation resin exchange bed is switched to the spare cation and cation resin exchange bed, and then the cation and cation resin exchange bed is subjected to alkaline acid regeneration treatment.
[0072] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present invention only and are not intended to limit the scope of the invention. The experimental methods in the following examples where specific conditions are not specified are generally measured in accordance with national standards. If there are no corresponding national standards, then the methods are carried out in accordance with general international standards, conventional conditions, or the conditions recommended by the manufacturer.
[0073] Example 1 This example provides a method for purifying an NMMO solvent recovery solution in a cellulose fiber prepared by an NMMO solvent process, the method comprising the following steps:
[0074] (1) A 1.5% foaming dilute solvent solution produced in the stock solution workshop, an 18% coagulation bath solution produced in the spinning workshop, and a commercially available flocculant, FLOPAM FO 4650, with a concentration of 0.15%, are added together into a solvent water recovery tank to adjust the NMMO concentration to 17%, wherein the flocculant concentration is 0.5%, and the mixture is stirred and mixed, and subjected to physical and chemical treatment;
[0075] (2) The 17% solution obtained in the solvent water recovery tank of step (1) was automatically backwashed through a disc filter with an accuracy of 150 μm at a rate of 50 m3 / h, with an automatic backwash pressure difference of 0.05 MPa and a backwash time of 10 seconds to remove most of the suspended matter, filaments and other solid impurities with a particle size of more than 150 μm;
[0076] (3) The NMMO solvent solution after primary filtration in step (2) is sequentially passed through a multi-media bed filter filled with pumice, quartz sand, and gravel from top to bottom, wherein the particle sizes are 2.5-3.5 mm, 0.50-1.50 mm, and 2.0-3.5 mm, respectively, and the filling heights are 1200 mm, 900 mm, and 300 mm, respectively, to remove suspended solids larger than 10 μm. The multi-media bed filter is backwashed and regenerated with a turbidimeter set to 1.0 NTU;
[0077] (4) The NMMO solvent solution obtained by filtration in step (3) is passed through a titanium fiber precision filter with a sintered felt filter element having a precision of 15 μm, 8 μm, and 3 μm from the outside to the inside, respectively, to remove suspended solids with a particle size of 3 μm or more;
[0078] (5) The NMMO solvent solution obtained by filtration in step (4) is passed through an anion resin bed filled with a macroporous strong basic anion exchange resin having a quaternary ammonium group introduced into a macroporous styrene-divinylbenzene polymer skeleton (a product of Xi'an Lanxiao Technology New Materials Co., Ltd., model LX-500, particle size 35 mesh, the filling amount of the anion exchange resin in the anion fixed bed is 70% of the volume of the exchange bed, and the flow rate of the NMMO solvent solution through the exchange bed is 4 BV / h) to remove organic colored groups, and the setting value of the resin regeneration colorimeter is 120 Hazen;
[0079] (6) The NMMO solvent solution obtained by filtration in step (5) is passed through a cationic resin bed filled with a strong acidic cation exchange resin having a macroporous structure and a sulfonic acid group introduced into a macroporous styrene-divinylbenzene polymer skeleton (a product of Xi'an Lanxiao Technology New Materials Co., Ltd., model LX-150, particle size 35 mesh, the filling amount of the cation exchange resin in the cation fixed bed is 50% of the volume of the exchange bed, and the flow rate of the 17% NMMO solvent solution through the exchange bed is 4 BV / h) to remove metal ions and morpholine and methylmorpholine. The set value of the resin regeneration conductivity is 30 μS / cm.
[0080] After testing, after 72 hours of continuous operation, the turbidity value of the purified NMMO solvent solution in this embodiment decreased from 2.6 NTU to 0.2 NTU, the color value decreased from 150 Hazen to 66 Hazen, and the conductivity decreased from 82 μS / cm to 3 μS / cm. The recovery rate of the NMMO solvent reached 98.8%.
[0081] Example 2
[0082] This example provides a method for purifying an NMMO solvent recovery solution in the preparation of cellulose fibers by an NMMO solvent process, the method comprising the following steps:
[0083] (1) A 2.5% foaming dilute solvent solution produced in the stock solution workshop, a 20% coagulation bath solution produced in the spinning workshop, and a commercially available flocculant of 0.15% are added to a solvent water recovery tank to adjust the concentration of NMMO to 17%, wherein the flocculant concentration is 0.8%, and the mixture is stirred and mixed, and subjected to physical and chemical treatment;
[0084] (2) The 17% solution obtained in the solvent water recovery tank of step (1) was automatically backwashed through a disc filter with an accuracy of 150 μm at a rate of 50 m3 / h, with an automatic backwash pressure difference of 0.05 MPa and a backwash time of 10 seconds to remove most of the suspended matter, filaments and other solid impurities with a particle size of more than 150 μm;
[0085] (3) The NMMO solvent solution after primary filtration in step (2) is sequentially passed through a multi-media bed filter filled with pumice, quartz sand, and gravel from top to bottom, wherein the particle sizes are 2.5-3.5 mm, 0.50-1.50 mm, and 2.0-3.5 mm, respectively, and the filling heights are 1200 mm, 900 mm, and 300 mm, respectively, to remove suspended solids larger than 10 μm. The multi-media bed filter is backwashed and regenerated with a turbidimeter set to 1.0 NTU;
[0086] (4) The NMMO solvent solution obtained by filtration in step (3) is passed through a titanium fiber precision filter with a sintered felt filter element having a precision of 15 μm, 8 μm, and 3 μm from the outside to the inside, respectively, to remove suspended solids with a particle size of 3 μm or more;
[0087] (5) The NMMO solvent solution obtained by filtration in step (4) is passed through an anion resin bed filled with a macroporous strong basic anion exchange resin (a product of Xi'an Lanxiao Technology New Materials Co., Ltd., model LX-500, particle size 35 mesh, the filling amount of the anion exchange resin in the anion fixed bed is 70% of the volume of the exchange bed, and the flow rate of the NMMO solvent solution through the exchange bed is 4 BV / h) to remove organic colored groups. The setting value of the resin regeneration colorimeter is 120 Hazen;
[0088] (6) The NMMO solvent solution obtained by filtration in step (5) is passed through a cationic resin bed filled with a strong acidic cation exchange resin having a macroporous structure and a sulfonic acid group introduced into a macroporous styrene-divinylbenzene polymer skeleton (a product of Xi'an Lanxiao Technology New Materials Co., Ltd., model LX-150, particle size 35 mesh, the filling amount of the cation exchange resin in the cation fixed bed is 50% of the volume of the exchange bed, and the flow rate of the 17% NMMO solvent solution through the exchange bed is 4 BV / h) to remove metal ions and morpholine and methylmorpholine. The set value of the resin regeneration conductivity is 30 μS / cm.
[0089] After testing, after 72 hours of continuous operation, the turbidity value of the purified NMMO solvent solution in this embodiment decreased from 2.7 NTU to 0.3 NTU, the color value decreased from 122 Hazen to 73 Hazen, and the conductivity decreased from 108 μS / cm to 4 μS / cm. The recovery rate of the NMMO solvent reached 98.7%.
[0090] Example 3
[0091] This example provides a method for purifying an NMMO solvent recovery solution in the preparation of cellulose fibers by an NMMO solvent process, the method comprising the following steps:
[0092] (1) A 4.5% foaming dilute solvent solution produced in the stock solution workshop, a 22% coagulation bath solution produced in the spinning workshop, and a commercially available flocculant, FLOPAM FO 4650, with a concentration of 0.15%, were added together into a solvent water recovery tank to adjust the NMMO concentration to 17%, wherein the flocculant concentration was 2.2%, and the mixture was stirred and mixed, and subjected to physical and chemical treatment;
[0093] (2) The 17% solution obtained in the solvent water recovery tank of step (1) was automatically backwashed through a disc filter with an accuracy of 150 μm at a rate of 50 m3 / h, with an automatic backwash pressure difference of 0.05 MPa and a backwash time of 10 seconds to remove most of the suspended matter, filaments and other solid impurities with a particle size of more than 150 μm;
[0094] (3) The NMMO solvent solution after primary filtration in step (2) is sequentially passed through a multi-media bed filter filled with pumice, quartz sand, and gravel from top to bottom, wherein the particle sizes are 2.5-3.5 mm, 0.50-1.50 mm, and 2.0-3.5 mm, respectively, and the filling heights are 1200 mm, 900 mm, and 300 mm, respectively, to remove suspended solids larger than 10 μm. The multi-media bed filter is backwashed and regenerated with a turbidimeter set to 1.0 NTU;
[0095] (4) The NMMO solvent solution obtained by filtration in step (3) is passed through a titanium fiber precision filter with a sintered felt filter element having a precision of 15 μm, 8 μm, and 3 μm from the outside to the inside, respectively, to remove suspended solids with a particle size of 3 μm or more;
[0096] (5) The NMMO solvent solution obtained by filtration in step (4) is passed through an anion resin bed filled with a macroporous strong basic anion exchange resin (a product of Xi'an Lanxiao Technology New Materials Co., Ltd., model LX-500, particle size 35 mesh, the filling amount of the anion exchange resin in the anion fixed bed is 70% of the volume of the exchange bed, and the flow rate of the NMMO solvent solution through the exchange bed is 4 BV / h) to remove organic colored groups. The setting value of the resin regeneration colorimeter is 120 Hazen;
[0097] (6) The NMMO solvent solution obtained by filtration in step (5) is passed through a cationic resin bed filled with a strong acidic cation exchange resin having a macroporous structure and a sulfonic acid group introduced into a macroporous styrene-divinylbenzene polymer skeleton (a product of Xi'an Lanxiao Technology New Materials Co., Ltd., model LX-150, particle size 35 mesh, the filling amount of the cation exchange resin in the cation fixed bed is 50% of the volume of the exchange bed, and the flow rate of the 17% NMMO solvent solution through the exchange bed is 4 BV / h) to remove metal ions and morpholine and methylmorpholine. The set value of the resin regeneration conductivity is 30 μS / cm.
[0098] After testing, after 72 hours of continuous operation, the turbidity value of the purified NMMO solvent solution in this embodiment decreased from 3.2 NTU to 0.5 NTU, the color value decreased from 142 Hazen to 93 Hazen, and the conductivity decreased from 136 μS / cm to 5 μS / cm. The recovery rate of the NMMO solvent reached 98.5%.
[0099] In summary, the embodiments of the present invention provide a method for purifying the NMMO solvent recovery solution in the preparation of cellulose fibers by the NMMO solvent method, by passing the collected recovered NMMO solvent aqueous solution through a multi-level, multi-media filter to effectively remove various impurities such as solid particles and metal ions, thereby achieving a process method for recovering and purifying the NMMO solvent solution.
[0100] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in a range format is only for convenience and brevity and should not be construed as an inflexible limitation on the scope of the invention; therefore, the range description should be considered to have specifically disclosed all possible subranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. In addition, whenever a numerical range is indicated herein, it is intended to include any cited numeral (fractional or integer) within the indicated range.
[0101] The foregoing description is intended only to provide specific embodiments of the present invention, which will enable those skilled in the art to understand and implement the present invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention is not intended to be limited to the embodiments shown herein, but is intended to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for purifying NMMO solvent recovery solution in the preparation of cellulose fiber by NMMO solvent method, characterized in that: The method comprises the following steps: Adding a flocculant to the NMMO solvent recovery solution to be treated for physical and chemical treatment to obtain a first NMMO solvent recovery solution; The first NMMO solvent recovery solution is sequentially subjected to solvent coarse filtration, multi-media bed filter and solvent fine filtration to obtain a second NMMO solvent recovery solution; subjecting the second NMMO solvent recovery solution to anion exchange treatment to obtain a third NMMO solvent recovery solution; The third NMMO solvent recovery solution is subjected to cation exchange treatment to obtain a purified NMMO solvent recovery solution.
2. The method for purifying the NMMO solvent recovery solution in the preparation of cellulose fiber by the NMMO solvent process according to claim 1, characterized in that: The method further comprises the following steps: The turbidity of the solution after filtration by the multi-media bed filter is detected by a turbidity meter, and if the turbidity value is greater than 1NTU, the multi-media bed filter is started to be regenerated; A colorimeter is used to detect the chromaticity of the solution after the anion exchange treatment. If the chromaticity value is greater than 100 Hazen, the anion resin exchange bed is started for regeneration; The conductivity of the solution after the cation exchange treatment is detected by a conductivity meter. If the conductivity is greater than 30 μS / cm, the cation resin exchange bed is started for regeneration.
3. The method for purifying the NMMO solvent recovery solution in the preparation of cellulose fiber by the NMMO solvent process according to claim 1, characterized in that: The NMMO solvent recovery solution to be processed includes: a foam dilute solvent solution produced in a stock solution workshop in the preparation of cellulose fibers by the NMMO solvent method, and a coagulation bath solution produced in a spinning workshop in the preparation of cellulose fibers by the NMMO solvent method; In terms of weight percentage, the NMMO concentration in the foam dilute solvent solution is 0.6-5%; In terms of weight percentage, the NMMO concentration in the coagulation bath solution is 15-25%.
4. The method for purifying the NMMO solvent recovery solution in the preparation of cellulose fiber by the NMMO solvent process according to claim 1, characterized in that: In terms of weight percentage, the added amount of the flocculant accounts for 0.5-2.5% of the entire material system; the model of the flocculant is FLOPAMFO4650.
5. The method for purifying the NMMO solvent recovery solution in the preparation of cellulose fiber by the NMMO solvent process according to claim 1, characterized in that: In terms of weight percentage, the concentration of the initial diluted solution to which the flocculant is added is 0.1-0.5%.
6. The method for purifying the NMMO solvent recovery solution in the preparation of cellulose fiber by the NMMO solvent process according to claim 1, characterized in that: The solvent coarse filtration adopts an automatic backwashing stacked disc filter. The working condition parameters of the automatic backwashing stacked disc filter include: using a polypropylene plastic filter plate with an accuracy of 150-250μm, a filtration backwashing pressure difference of 0.02-0.05MPa or a set time of 1.5-2.5 hours, and a backwashing completion time of 10-30 seconds.
7. The method for purifying the NMMO solvent recovery solution in the preparation of cellulose fibers by the NMMO solvent process according to claim 1, characterized in that: The filter media of the multi-media bed filter are filled from top to bottom with pumice with a particle size of 2.5-3.5 mm, quartz sand with a particle size of 0.50-1.50 mm, and gravel with a particle size of 2.0-3.5 mm, respectively, and the stacking heights of the filter media layers are 1200 mm, 900 mm, and 300 mm.
8. The method for purifying NMMO solvent recovery solution in preparing cellulose fiber by NMMO solvent process according to claim 1, characterized in that: The solvent fine filtration adopts a titanium fiber precision filter, and the working condition parameters of the titanium fiber precision filter include: the filter element adopts sintered felt, and its filtration accuracy from outside to inside is 3μm, 8μm, 15μm, and 30μm respectively.
9. The method for purifying NMMO solvent recovery solution in preparing cellulose fiber by NMMO solvent process according to claim 1, characterized in that: The anion exchange treatment adopts an anion fixed bed filled with anion exchange resin, the filling amount of the anion exchange resin in the anion fixed bed is 30-80% of the volume of the exchange bed, and the flow rate of the purified solution containing N-methylmorpholine N-oxide passing through the exchange bed is 3-6BV / h; the anion exchange resin is a macroporous, strongly alkaline, epoxy-based anion exchange resin with -OH groups, and the particle size of the epoxy-based anion exchange resin is 20-40 meshes.
10. The method for purifying NMMO solvent recovery solution in preparing cellulose fibers by NMMO solvent process according to claim 1, characterized in that: The cationic treatment adopts a cationic fixed bed filled with cationic exchange resin, the filling amount of the cationic exchange resin in the cationic fixed bed is 30-80% of the volume of the exchange bed, the flow rate of the purified solution containing N-methylmorpholine N-oxide passing through the exchange bed is 3-6BV / h, the cationic exchange resin is a macroporous strongly acidic propylene-based cation exchange resin with a -H group, and the particle size of the propylene-based cation exchange resin is 20-40 meshes.
Citation Information
Patent Citations
Recovery method of N-methylmorpholine oxide solvent in process of producing regenerated cellulose fibre by solvent method
CN101942712A
Purification method of Lyocell spinning coagulating bath recovery liquid
CN111943340A
Process for purifying tertiary aminoxide aqueous solution
CN1163639A
Solvent recovery process for solvent method cellulose fiber preparation
CN1603479A
Cited By
NMMO (N-methylmorpholine-N-oxide) waste glue solution recycling system in lyocell fiber production
CN120717660A