Wear-resistant glass fiber and preparation method thereof

By adding molybdenum dioxide and coupling agent to the preparation of glass fibers to form a mesh structure, and combining acid leaching treatment, the problem of insufficient brittleness and wear resistance of glass fibers is solved, and glass fibers with high wear resistance and low brittleness are achieved , suitable for high demanding industrial applications.

CN119080398AInactive Publication Date: 2024-12-06JIANGSU KELU NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187196.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Glass fibers are prone to break when impacted by external forces or bent, and have poor wear resistance, which limits their application in situations where high flexibility and impact resistance are required, especially in fields such as ships, automobiles, construction and industrial manufacturing.

Method used

By adding molybdenum dioxide, coupling agent and film forming agent to the preparation method, a solid mesh structure is formed, combined with acid leach treatment, the wear resistance of glass fibers is improved and the brittleness is reduced. The process steps include melting, drawing and cooling treatment. .

Benefits of technology

It achieves high wear resistance and low brittleness of glass fiber, enhances its insulation, heat resistance and corrosion resistance, and improves the purity and surface quality of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013853760000061
    Figure BDA0005013853760000061
Patent Text Reader

Abstract

The invention relates to the technical field of glass fibers, in particular to a wear-resistant glass fiber and a preparation method thereof. The invention provides a wear-resistant glass fiber. The wear-resistant glass fiber comprises the following raw materials: 55-65% of silicon dioxide, 10-15% of aluminum oxide, 2-3% of boric oxide, 0.5-1.0% of sodium oxide, 1.5-2.0% of molybdenum dioxide, 6-11% of a film-forming agent, 3-7% of a coupling agent, 1-2% of a pH regulator and 3-5% of a defoaming agent. The preparation method comprises the following three steps: S1, melting; S2, forming a glass fiber precursor; and S3, generating the glass fiber. The glass fiber finished product prepared by the method not only has good insulativity, heat resistance and corrosion resistance, but also has higher wear resistance and lower brittleness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass fibers, and in particular to a wear-resistant glass fiber and a preparation method thereof. Background Art

[0002] Glass fiber is an inorganic non-metallic material with excellent performance. It has a wide variety of advantages, such as good insulation, strong heat resistance, good corrosion resistance, and high mechanical strength. Therefore, it is usually used as a reinforcing material in composite materials, electrical insulation materials, and thermal insulation materials, and is used in many fields. However, glass fiber still cannot meet the needs of some industries, because glass fiber is brittle and easily breaks when impacted or bent by external forces, which limits its application in certain occasions that require high flexibility and impact resistance; it has poor wear resistance, and long-term friction or wear will cause damage to the surface of the glass fiber, affecting its performance and life.

[0003] Glass fiber with high wear resistance plays an important role in many fields such as shipbuilding and marine engineering, automotive industry, construction and infrastructure, industrial manufacturing, and energy industry. These industries have very high requirements on the wear resistance of materials, so it is necessary to invent a glass fiber with high wear resistance. Summary of the invention

[0004] In view of the above-mentioned existing technical problems, the present invention aims to provide a wear-resistant glass fiber and a preparation method thereof. The glass fiber prepared by this method has good insulation, heat resistance, high wear resistance and low brittleness.

[0005] The present invention discloses a wear-resistant glass fiber, comprising the following components in parts by weight:

[0006] Silicon dioxide 55-70.4%, aluminum oxide 10-15%, boron oxide 2-3%, sodium oxide 0.5-1.0%, molybdenum dioxide 1.5-2.0%, film-forming agent 6-11%, coupling agent 3-7%, pH adjuster 1-2%, defoaming agent 3-5%.

[0007] Preferably, the film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1:(0.8-1.0).

[0008] Preferably, the coupling agent is aminosilane and siloxane in a mass ratio of 1: (3-4).

[0009] The present invention also discloses a method for preparing wear-resistant glass fiber, which comprises the following process steps:

[0010] S1 melting: Add the prepared raw materials of silicon dioxide, aluminum oxide, boron oxide, sodium oxide, molybdenum dioxide and coupling agent into the pool kiln in proportion, heat to a molten state, react for a period of time, and then add pH adjuster, film-forming agent and defoaming agent to the molten mixture in the pool kiln in turn, stir and mix, and after the reaction is completed, a molten glass liquid is obtained.

[0011] S2 forms glass fiber strands: the molten glass obtained in step S1 is drawn at high speed from a leak plate connected to the tank kiln into continuous glass fiber strands.

[0012] S3 generates glass fiber: the glass fiber raw yarn obtained in step S2 is cooled and acid-impregnated to obtain glass fiber.

[0013] Preferably, in the S1 melting step, the heating temperature is 1000-1100°C.

[0014] Preferably, in the S1 melting step, the reaction time is 3 to 5 hours.

[0015] Preferably, in the step S2 of forming glass fiber precursor, the speed during the drawing process is 2300-2500 m / min.

[0016] Preferably, in the step S2 of forming glass fiber precursors, the number of holes of the leaking plate is 1000 to 1200.

[0017] Preferably, in the S2 coagulant preparation step, the rotary evaporation method is reduced-pressure rotary evaporation; and the drying method is freeze-drying.

[0018] Preferably, in the step of generating glass fibers in S3, the temperature is lowered to 20-30° C. during the cooling process.

[0019] Preferably, in the step of generating glass fibers in S3, the acid solution used in the acid leaching process is a sulfuric acid solution with a mass fraction of 3 to 5%.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The glass fiber provided by the invention has good insulation, heat resistance and corrosion resistance, as well as high wear resistance and low brittleness. This is because a certain proportion of molybdenum dioxide is added to the raw material of the glass fiber. The octahedral structure of molybdenum dioxide in the molten state can form a solid mesh structure with other metal oxides under the action of the improved coupling agent, and then react with the improved film-forming agent to form a film on the metal mesh, which can effectively improve the wear resistance of the finished glass fiber and reduce the brittleness of the glass fiber to a certain extent. In this process, the pH regulator needs to be heated to control the pH value of the molten mixture.

[0022] The present invention also provides a method for preparing wear-resistant glass fiber. The raw materials are added in two steps to make the reaction more complete and the formed network structure more stable. After cooling, an acid leaching process is performed to remove some impurities on the surface of the glass fiber and improve the purity and surface quality of the glass fiber. DETAILED DESCRIPTION

[0023] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0024] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0025] Embodiment 1: A wear-resistant glass fiber, composed of the following components in parts by weight:

[0026] Silicon dioxide 55%, aluminum oxide 15%, boron oxide 3%, sodium oxide 1.0%, molybdenum dioxide 2.0%, film-forming agent 11%, coupling agent 7%, pH adjuster 2%, defoaming agent 4%.

[0027] The film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1:0.8; the coupling agent is composed of aminosilane and siloxane in a mass ratio of 1:3.

[0028] A method for preparing wear-resistant glass fiber comprises the following process steps:

[0029] S1 melting: the above-prepared raw materials of 55% silicon dioxide, 15% aluminum oxide, 3% boron oxide, 1.0% sodium oxide, 2.0% molybdenum dioxide and 7% coupling agent are added into the pool kiln in proportion, heated to 1000°C until molten, react for 0.5h, and then 2% pH adjuster, 11% film-forming agent and 4% defoaming agent are added into the molten mixture in the pool kiln in turn, and stirred and mixed. During the reaction, the pH of the molten glass liquid is stabilized between 7.0 and 7.5. After reacting for 2.5h, molten glass liquid is obtained.

[0030] S2: Forming glass fiber precursor: The molten glass obtained in step S1 is drawn from a bushing connected to the tank kiln at a high speed of 2300 m / min into continuous glass fiber precursor. The bushing has 1000 holes.

[0031] S3 generates glass fiber: the glass fiber precursor obtained in step S2 is cooled at a cooling temperature of 20-30° C. After the glass fiber precursor is cooled, it is placed in a sulfuric acid solution with a mass fraction of 3-5% for acid leaching to finally obtain glass fiber.

[0032] Embodiment 2: A wear-resistant glass fiber, composed of the following components in parts by weight:

[0033] Silicon dioxide 57.6%, aluminum oxide 14%, boron oxide 2.8%, sodium oxide 0.9%, molybdenum dioxide 1.9%, film-forming agent 10%, coupling agent 6%, pH adjuster 1.8%, defoaming agent 5%.

[0034] The film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1:0.85; the coupling agent is composed of aminosilane and siloxane in a mass ratio of 1:3.2.

[0035] A method for preparing wear-resistant glass fiber comprises the following process steps:

[0036] S1 melting: the above-prepared raw materials of 57.6% silicon dioxide, 14% aluminum oxide, 2.8% boron oxide, 0.9% sodium oxide, 1.9% molybdenum dioxide and 6% coupling agent are added into the pool kiln in proportion, heated to 1120°C until molten, reacted for 0.75h, and then 1.8% pH adjuster, 10% film-forming agent and 5% defoaming agent are added into the molten mixture in the pool kiln in turn, stirred and mixed, during the reaction, the pH of the molten glass liquid is stabilized between 7.0 and 7.5, and after reacting for 2.7.5h, molten glass liquid is obtained.

[0037] S2 Forming glass fiber precursor: The molten glass obtained in step S1 is drawn from a bushing connected to the tank kiln at a high speed of 2350 m / min into continuous glass fiber precursor. The bushing has 1050 holes.

[0038] S3 generates glass fiber: the glass fiber precursor obtained in step S2 is cooled at a cooling temperature of 20-30° C. After the glass fiber precursor is cooled, it is placed in a sulfuric acid solution with a mass fraction of 3-5% for acid leaching to finally obtain glass fiber.

[0039] Embodiment 3: A wear-resistant glass fiber, comprising the following components in parts by weight:

[0040] Silicon dioxide 61.7%, aluminum oxide 13%, boron oxide 2.6%, sodium oxide 0.8%, molybdenum dioxide 1.8%, film-forming agent 9%, coupling agent 5%, pH adjuster 1.6%, defoaming agent 4.5%.

[0041] The film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1:0.9; the coupling agent is composed of aminosilane and siloxane in a mass ratio of 1:3.4.

[0042] A method for preparing wear-resistant glass fiber comprises the following process steps:

[0043] S1 melting: the above-prepared raw materials of 61.7% silicon dioxide, 13% aluminum oxide, 2.6% boron oxide, 0.8% sodium oxide, 1.8% molybdenum dioxide and 5% coupling agent are added into the pool kiln in proportion, heated to 1140°C until molten state, reacted for 1.0h, and then 1.6% pH adjuster, 9% film-forming agent and 4.5% defoaming agent are added into the molten mixture in the pool kiln in turn, stirred and mixed, during the reaction, the pH of the molten glass liquid is stabilized between 7.0 and 7.5, and after reacting for 3.0h, molten glass liquid is obtained.

[0044] S2 Forming glass fiber precursor: The molten glass obtained in step S1 is drawn from a bushing connected to the tank kiln at a high speed of 2400 m / min into continuous glass fiber precursor. The bushing has 1100 holes.

[0045] S3 generates glass fiber: the glass fiber precursor obtained in step S2 is cooled at a cooling temperature of 20-30° C. After the glass fiber precursor is cooled, it is placed in a sulfuric acid solution with a mass fraction of 3-5% for acid leaching to finally obtain glass fiber.

[0046] Embodiment 4: A wear-resistant glass fiber, composed of the following components in parts by weight:

[0047] Silicon dioxide 66.3%, aluminum oxide 12%, boron oxide 2.4%, sodium oxide 0.7%, molybdenum dioxide 1.7%, film-forming agent 8%, coupling agent 4%, pH adjuster 1.4%, defoaming agent 3.5%.

[0048] The film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1:0.95; the coupling agent is composed of aminosilane and siloxane in a mass ratio of 1:3.6.

[0049] A method for preparing wear-resistant glass fiber comprises the following process steps:

[0050] S1 melting: the above-prepared raw materials of 66.3% silicon dioxide, 12% aluminum oxide, 2.4% boron oxide, 0.7% sodium oxide, 1.7% molybdenum dioxide and 4% coupling agent are added into the pool kiln in proportion, heated to 1160°C until molten, reacted for 1.25h, and then 1.4% pH adjuster, 8% film-forming agent and 3.5% defoaming agent are added into the molten mixture in the pool kiln in turn, stirred and mixed, during the reaction, the pH of the molten glass liquid is stabilized between 7.0 and 7.5, and after reacting for 3.25h, molten glass liquid is obtained.

[0051] S2 Forming glass fiber precursor: The molten glass obtained in step S1 is drawn from a bushing connected to the tank kiln at a high speed of 2450 m / min into continuous glass fiber precursor. The bushing has 1150 holes.

[0052] S3 generates glass fiber: the glass fiber precursor obtained in step S2 is cooled at a cooling temperature of 20-30° C. After the glass fiber precursor is cooled, it is placed in a sulfuric acid solution with a mass fraction of 3-5% for acid leaching to finally obtain glass fiber.

[0053] Embodiment 5: A wear-resistant glass fiber, composed of the following components in parts by weight:

[0054] Silicon dioxide 70.4%, aluminum oxide 11%, boron oxide 2.2%, sodium oxide 0.6%, molybdenum dioxide 1.6%, film-forming agent 7%, coupling agent 3%, pH adjuster 1.2%, defoaming agent 3.0%.

[0055] The film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1:1.0; the coupling agent is composed of aminosilane and siloxane in a mass ratio of 1:4.0.

[0056] A method for preparing wear-resistant glass fiber comprises the following process steps:

[0057] S1 melting: the above-prepared raw materials of silicon dioxide 70.4%, aluminum oxide 11%, boron oxide 2.2%, sodium oxide 0.6%, molybdenum dioxide 1.6%, and coupling agent 3% are added into the pool kiln in proportion, heated to 1200°C until molten state, reacted for 1.5 hours, and then pH adjuster 1.2%, film-forming agent 7% and defoaming agent 3.0% are added into the molten mixture in the pool kiln in turn, stirred and mixed, during the reaction, the pH of the molten glass liquid is stabilized between 7.0 and 7.5, and after reacting for 3.5 hours, molten glass liquid is obtained.

[0058] S2 Forming glass fiber precursor: The molten glass obtained in step S1 is drawn from a bushing connected to the tank kiln at a high speed of 2500 m / min into continuous glass fiber precursor. The bushing has 1200 holes.

[0059] S3 generates glass fiber: the glass fiber precursor obtained in step S2 is cooled at a cooling temperature of 20-30° C. After the glass fiber precursor is cooled, it is placed in a sulfuric acid solution with a mass fraction of 3-5% for acid leaching to finally obtain glass fiber.

[0060] Comparative Example 1: No molybdenum dioxide was added to the raw materials, and the remaining raw material amounts, reaction conditions, and reaction steps were the same as those in Example 4.

[0061] Comparative Example 2: The coupling agent in the raw materials is composed entirely of aminosilane, and the amounts of other raw materials, reaction conditions and reaction steps are the same as those in Example 4.

[0062] Comparative Example 3: The coupling agent in the raw materials is composed entirely of siloxane, and the amounts of other raw materials, reaction conditions and reaction steps are the same as those in Example 4.

[0063] Comparative Example 4: The film-forming agent in the raw materials is entirely composed of polyvinyl acetate, and the amounts of other raw materials, reaction conditions and reaction steps are the same as those in Example 4.

[0064] Comparative Example 5: The film-forming agent in the raw materials is entirely composed of polyurethane, and the amounts of other raw materials, reaction conditions and reaction steps are the same as those in Example 4.

[0065] The finished glass fibers prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were tested, and the experimental data are shown in the following table:

[0066]

[0067] As can be seen from the table above, the wear amount of Examples 1 to 5 is much lower than that of Comparative Examples 1 to 5 from the experimental data, the compressive strength of the Examples is stronger, the expansion coefficient and dielectric constant are smaller, and the density is more uniform. In Comparative Examples 1 to %, no molybdenum dioxide, aminosilane,

[0068] Silicone, polyvinyl acetate and polyurethane, so no stable network structure is formed, resulting in the final glass fiber product having low wear resistance and low compressive strength; it is obviously affected by temperature, the expansion coefficient is too large, the dielectric constant is also too large, the possibility of being polarized in the magnetic field is high, it is not sufficiently insulated, and there is a risk of conductivity; the finished products of Examples 1 to 5 have a more uniform density, a smaller deviation, and are more stable.

[0069] In summary, the finished product obtained by the wear-resistant glass fiber and the preparation method thereof provided by the present invention has good insulation, heat resistance and corrosion resistance, as well as high wear resistance and low brittleness. Among them, the preparation conditions and raw material ratios of Example 4 are the best.

[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A wear-resistant glass fiber, It is characterized in that The composition comprises the following components in parts by weight: Silicon dioxide 55-70.4%, aluminum oxide 10-15%, boron oxide 2-3%, sodium oxide 0.5-1.0%, molybdenum dioxide 1.5-2.0%, film-forming agent 6-11%, coupling agent 3-7%, pH adjuster 1-2%, defoaming agent 3-5%.

2. A wear-resistant glass fiber according to claim 1, It is characterized in that The film-forming agent is composed of polyvinyl acetate and polyurethane in a mass ratio of 1: (0.8-1.0).

3. The wear-resistant glass fiber according to claim 1, It is characterized in that The coupling agent is composed of aminosilane and siloxane in a mass ratio of 1: (3-4).

4. A method for preparing wear-resistant glass fiber, It is characterized in that The process steps include: S1 Melting: Add the prepared raw materials of silicon dioxide, aluminum oxide, boron oxide, sodium oxide, molybdenum dioxide and coupling agent into the tank kiln in proportion, heat them to a molten state, react for a period of time, then add a pH regulator, a film-forming agent and a defoaming agent to the molten mixture in the tank kiln in turn, stir and mix, and after the reaction is completed, obtain a molten glass liquid; S2 forming glass fiber precursor: the molten glass obtained in step S1 is drawn at high speed from a bushing connected to the tank kiln into continuous glass fiber precursor; S3 generates glass fiber: the glass fiber raw yarn obtained in step S2 is cooled and acid-impregnated to obtain glass fiber.

5. The method for preparing a wear-resistant glass fiber according to claim 4, It is characterized in that In the S1 melting step, the heating temperature is 1000-1100°C.

6. The method for preparing a wear-resistant glass fiber according to claim 4, It is characterized in that In the S1 melting step, the reaction time is 3 to 5 hours.

7. The method for preparing a wear-resistant glass fiber according to claim 4, It is characterized in that In the step S2 of forming glass fiber precursor, the speed during the drawing process is 2300-2500 m / min.

8. The method for preparing a wear-resistant glass fiber according to claim 4, It is characterized in that In the step S2 of forming glass fiber precursor, the number of holes of the bushing is 1000 to 1200.

9. The method for preparing a wear-resistant glass fiber according to claim 4, It is characterized in that In the step of generating glass fibers in S3, the temperature is lowered to 20-30°C during the cooling process.

10. The method for preparing a wear-resistant glass fiber according to claim 4, It is characterized in that In the step S3 of generating glass fibers, the acid solution used in the acid leaching process is a sulfuric acid solution with a mass fraction of 3 to 5%.