Anti-crack recycled concrete material and preparation method thereof
By using composite fiber anti-cracking agents and modifiers to fill the cracks and voids of fine aggregates in recycled concrete materials, the problems of insufficient crack resistance, compression resistance and permeability of existing recycled concrete materials are solved, and their performance is significantly improved and use safety.
Patent Information
- Application Number
- CN202411251334.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The crack resistance, compression resistance, dismantling resistance and permeability of existing recycled concrete materials are poor, resulting in lower safety in use.
Using composite fiber anti-cracking agent and modifier, the composite fiber anti-cracking agent is made by mixing expansion agent, dispersant, plant fiber, polypropylene fiber and water retention agent, combined with slag micropowder solvent and water glass solvent to regenerate fine collection. The material is modified to fill cracks and voids on its surface to improve crack resistance and permeability.
It significantly improves the crack resistance, compressive strength and demolition strength of recycled concrete, reduces water absorption, enhances permeability and frost resistance, and improves construction efficiency and use safety.
Smart Images

Figure CN119080448A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of crack-resistant recycled concrete, in particular to a crack-resistant recycled concrete material and a preparation method thereof. Background Art
[0002] Recycled concrete refers to new concrete made by crushing, cleaning, and grading discarded concrete blocks, mixing them with grading in a certain proportion, partially or completely replacing natural aggregates such as sand and gravel, and then adding cement, water, etc. The new concrete made directly has high discreteness and is prone to a large number of cracks, which leads to lower safety in the use of recycled concrete.
[0003] The existing defects are: 1. Patent document JP2009000606A discloses a device and method for recycling concrete waste. However, in the above document, the prepared recycled concrete has poor crack resistance and is prone to cracks during use. 2. Patent document JP2012025631A discloses recycled concrete of composite materials recovered from waste concrete as main materials, a method for manufacturing the same, and a method for treating waste concrete, for obtaining recycled materials. However, in the above document, there is a technical problem that the prepared recycled concrete has poor compressive strength and demolition resistance. 3. Patent document KR101385794B1 discloses a cement MORTAR PEELING OFF recycling method. However, in the above document, the recycled fine aggregate used has strong water absorption, which easily leads to the technical problem that the recycled concrete material prepared using the recycled fine aggregate has poor anti-permeability; 4. Patent document CN113321470B discloses a high-strength recycled concrete and a preparation method thereof. However, in the above document, there is a lack of materials for filling cracks and gaps on the surface of recycled fine aggregates, which easily leads to the technical problem that the prepared recycled concrete material has low strength. Summary of the invention
[0004] The object of the present invention is to provide a crack-resistant recycled concrete material and a preparation method thereof, so as to solve the technical problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a crack-resistant recycled concrete material, which is made of the following raw materials in parts by weight: 18-33 parts of a modifier, 33-50 parts of recycled aggregate, 37-50 parts of cement, 1-3 parts of a water reducer, 8-12 parts of a composite fiber anti-cracking agent, 13-23 parts of water, and 20-28 parts of sand; The modifier comprises the following raw materials in parts by weight: 6-11 parts of slag powder solvent, 6-11 parts of water glass solvent and 6-11 parts of polyvinyl alcohol solvent; The composite fiber anti-cracking agent is made of the following raw materials: expansion agent, dispersant, plant fiber, polypropylene fiber and water retaining agent, and the raw materials are mixed in the following mass percentages: expansion agent 95-99%, dispersant 0.2-1%, plant fiber 0.2-1%, polypropylene raw material 0.4-2% and water retaining agent 0.2-1%.
[0006] Preferably, the steps for preparing the crack-resistant recycled concrete material are as follows: S1. Grinding and crushing the recycled aggregate to obtain recycled fine aggregate; S2, soaking the recycled fine aggregate obtained in S1 in 6-11 parts of slag powder solvent for 1-2 hours, then taking it out and air-drying it, soaking the air-dried recycled fine aggregate in 6-11 parts of water glass solvent for 1-2 hours, then taking it out and air-drying it again, thereby obtaining the recycled fine aggregate No. 1 modified test sample; S3, after the plant fiber and the polypropylene fiber are evenly mixed, they are added into a twin-screw extruder for melting, extrusion, and drawing to obtain composite fibers, and then the obtained composite fibers are put into a cutting machine for crushing and cutting to obtain short-cut composite fibers; S4, mixing and stirring the chopped composite fibers obtained in S3 with the expansion agent, dispersant and water-retaining agent, and obtaining the desired composite fiber anti-cracking agent after the mixture is evenly mixed; S5, mixing the modified test sample No. 1 of recycled fine aggregate obtained in S2 with sand to obtain a mixture; S6, adding the composite fiber anti-cracking agent obtained in S4 to the preliminary mixture obtained in S5, and then mixing and stirring, and after the mixture is evenly mixed, a mixture containing the composite fiber anti-cracking agent is obtained; S7. Finally, cement, water reducing agent and water are added to the mixture with composite fiber anti-cracking agent added obtained in S5, and mixed and stirred. After being mixed evenly, the desired anti-cracking recycled concrete material is finally obtained.
[0007] Preferably, the recycled fine aggregate obtained by crushing in S1 has a particle diameter of less than 30 mm.
[0008] Preferably, the same mass of recycled fine aggregate is soaked in different modifiers in sequence according to the method in S2, thereby obtaining modified test samples of a variety of recycled fine aggregates, and the soaking time of the recycled fine aggregate in different modifiers is 1-2 hours.
[0009] Preferably, in S3, the polypropylene raw material is put into a twin-screw extruder, and the extrusion temperature when using the twin-screw extruder is 180-220° C. and the rotation speed of the twin-screw extruder is 320-400 rpm.
[0010] Preferably, the polypropylene fibers obtained after melting, extrusion and drawing in S3 are put into a cutting machine for cutting to obtain short-cut polypropylene fibers with a diameter of 8-12 μm and a length of 4-9 mm.
[0011] Preferably, the equipment for mixing and obtaining the composite fiber anti-cracking agent in S4 has a rotation speed of 500-750rpm and a mixing time of 45-60min, wherein the swelling agent is one of calcium oxide swelling agents, calcium sulfoaluminate swelling agents or magnesium oxide swelling agents, the dispersant is one of sodium tripolyphosphate, sodium hexametaphosphate or sodium pyrophosphate, and the water retaining agent is polyacrylamide.
[0012] Preferably, the rotation speed of the modified test sample No. 1 of recycled fine aggregate in S5 when mixed with sand is 400-800 rpm, and the mixing time is 0.5-1 h.
[0013] Preferably, the composite fiber anti-cracking agent in S6 is added to the preliminary mixture obtained in S5 at a mixing speed of 400-800 rpm and a mixing time of 0.5-1 h.
[0014] Preferably, when the desired anti-cracking recycled concrete material is obtained in S7, the mixing speed is 800-1200 rpm and the mixing time is 1-2 hours.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention adds a composite fiber anti-cracking agent to the recycled concrete material. The composite fiber anti-cracking agent has two anti-cracking components, namely, an expansion agent and composite fibers. It can improve the anti-cracking ability of the recycled concrete from both physical and chemical aspects, provide double protection for the concrete, and thus significantly improve the anti-cracking performance of the recycled concrete material. 2. The present invention prepares a composite fiber anti-cracking agent by mixing an expansion agent, a dispersant, plant fiber, polypropylene fiber and a water retaining agent. The composite fiber anti-cracking agent has the common advantages of an expansion agent and a composite fiber, can effectively solve the cracking and leakage problems of concrete engineering, and can realize the seamless construction of ultra-long structures. The prepared recycled concrete material has good compressive strength and demolition resistance, thereby improving the construction efficiency and the safety of the use of recycled concrete materials. 3. The present invention uses slag powder solvent to fill the cracks and gaps on the surface of the recycled fine aggregate with slag powder, and then uses water glass solvent and polyvinyl alcohol solvent to cover a thin film on the surface of the recycled fine aggregate, thereby reducing the water absorption rate of the recycled fine aggregate, thereby improving the anti-permeability and anti-freezing properties of the recycled concrete prepared with the recycled fine aggregate; 4. In the present invention, the more slag powder solvent participates in the modification, the higher the strength of the modified test sample of the recycled fine aggregate. The water glass solvent and the polyvinyl alcohol solvent can be mixed to form a gelling substance, which not only has a sticky effect, but also can fill in the cracks and gaps on the surface of the recycled fine aggregate, thereby improving the strength of the modified test sample of the recycled fine aggregate. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the preparation process of the present invention. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1: Please refer to Figure 1 , an embodiment provided by the present invention: a crack-resistant recycled concrete material is made of the following raw materials in parts by weight: including 18-33 parts of a modifier, 33-50 parts of recycled aggregate, 37-50 parts of cement, 1-3 parts of a water reducer, 8-12 parts of a composite fiber anti-cracking agent, 13-23 parts of water, and 20-28 parts of sand; The modifier comprises the following raw materials in parts by weight: 6-11 parts of slag powder solvent, 6-11 parts of water glass solvent and 6-11 parts of polyvinyl alcohol solvent; The composite fiber anti-cracking agent is made of the following raw materials: an expander, a dispersant, a plant fiber, a polypropylene fiber and a water retaining agent, and the mass percentage of the raw materials is: 95-99% of the expander, 0.2-1% of the dispersant, 0.2-1% of the plant fiber, 0.4-2% of the polypropylene raw material and 0.2-1% of the water retaining agent; The preparation steps of the anti-cracking recycled concrete material are as follows: S1. Grinding and crushing the recycled aggregate to obtain recycled fine aggregate; S2, soaking the recycled fine aggregate obtained in S1 in 6 parts of slag powder solvent for 1-2 hours, then taking it out and air-drying it, soaking the air-dried recycled fine aggregate in 6 parts of water glass solvent for 1-2 hours, then taking it out and air-drying it again, thereby obtaining the recycled fine aggregate No. 1 modified test sample; S3, after the plant fiber and the polypropylene fiber are evenly mixed, they are added into a twin-screw extruder for melting, extrusion, and drawing to obtain composite fibers, and then the obtained composite fibers are put into a cutting machine for crushing and cutting to obtain short-cut composite fibers; S4, mixing and stirring the chopped composite fibers obtained in S3 with the expansion agent, dispersant and water-retaining agent, and obtaining the desired composite fiber anti-cracking agent after the mixture is evenly mixed; S5, mixing the modified test sample No. 1 of recycled fine aggregate obtained in S2 with sand to obtain a mixture; S6, adding the composite fiber anti-cracking agent obtained in S4 to the preliminary mixture obtained in S5, and then mixing and stirring, and after the mixture is evenly mixed, a mixture containing the composite fiber anti-cracking agent is obtained; S7, finally, adding cement, water reducing agent and water into the mixture with the composite fiber anti-cracking agent added in S5, mixing and stirring, and finally obtaining the desired anti-cracking recycled concrete material after mixing evenly; The recycled fine aggregate obtained by crushing in S1 has a particle diameter of less than 30 mm; According to the method in S2, the recycled fine aggregate of the same mass is sequentially immersed in different modifiers, thereby obtaining modified test samples of various recycled fine aggregates, and the immersion time of the recycled fine aggregate in different modifiers is 1-2 hours; In S3, the polypropylene raw material is put into a twin-screw extruder, and the extrusion temperature of the twin-screw extruder is 180-220° C. and the rotation speed of the twin-screw extruder is 320-400 rpm; The polypropylene fibers obtained after melting, extrusion and drawing in S3 are put into a cutting machine for cutting to obtain short-cut polypropylene fibers with a diameter of 8-12 μm and a length of 4-9 mm; The equipment for mixing and obtaining the composite fiber anti-cracking agent in S4 has a rotation speed of 500-750 rpm and a mixing time of 45-60 min, wherein the expansion agent is one of a calcium oxide expansion agent, a calcium sulfoaluminate expansion agent or a magnesium oxide expansion agent, the dispersant is one of sodium tripolyphosphate, sodium hexametaphosphate or sodium pyrophosphate, and the water retaining agent is polyacrylamide; The speed of mixing the modified test sample No. 1 of recycled fine aggregate with sand in S5 was 400-800 rpm and the mixing time was 0.5-1 h; The composite fiber anti-cracking agent in S6 is added to the preliminary mixture obtained in S5 at a mixing speed of 400-800 rpm and a mixing time of 0.5-1 h; When the desired anti-cracking recycled concrete material is obtained in S7, the mixing speed is 800-1200 rpm and the mixing time is 1-2 hours.
[0019] Example 2: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of slag powder solvent for 1-2 hours and then taken out and air-dried, and the air-dried recycled fine aggregate is soaked in 11 parts of water glass solvent for 1-2 hours and then taken out and air-dried again, thereby obtaining the recycled fine aggregate No. 2 modified test sample.
[0020] Example 3: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 6 parts of slag powder solvent for 1-2 hours and then taken out and air-dried, and the air-dried recycled fine aggregate is soaked in 6 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out and air-dried again, thereby obtaining the recycled fine aggregate No. 3 modified test sample.
[0021] Example 4: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of slag powder solvent for 1-2 hours and then taken out and air-dried, and the air-dried recycled fine aggregate is soaked in 11 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out and air-dried again, thereby obtaining the recycled fine aggregate No. 4 modified test sample.
[0022] Example 5: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 6 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out and air-dried, and the air-dried recycled fine aggregate is soaked in 6 parts of water glass solvent for 1-2 hours and then taken out and air-dried again, thereby obtaining the recycled fine aggregate No. 5 modified test sample.
[0023] Example 6: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out and air-dried, and the air-dried recycled fine aggregate is soaked in 11 parts of water glass solvent for 1-2 hours and then taken out and air-dried again, thereby obtaining the recycled fine aggregate No. 6 modified test sample.
[0024] Example 7: Please refer to Figure 1An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 6 parts of slag powder solvent for 1-2 hours and then taken out for air-drying, the air-dried recycled fine aggregate is soaked in 6 parts of water glass solvent for 1-2 hours and then taken out for air-drying again, and finally the air-dried recycled fine aggregate is soaked in 6 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air-drying again, thereby obtaining the recycled fine aggregate No. 7 modified test sample.
[0025] Example 8: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 6 parts of slag powder solvent for 1-2 hours and then taken out for air-drying, the air-dried recycled fine aggregate is soaked in 6 parts of water glass solvent for 1-2 hours and then taken out for air-drying again, and finally the air-dried recycled fine aggregate is soaked in 11 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air-drying again, thereby obtaining the recycled fine aggregate No. 8 modified test sample.
[0026] Example 9: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 6 parts of slag powder solvent for 1-2 hours and then taken out for air drying, the air-dried recycled fine aggregate is soaked in 11 parts of water glass solvent for 1-2 hours and then taken out for air drying again, and finally the air-dried recycled fine aggregate is soaked in 11 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air drying again, thereby obtaining the recycled fine aggregate No. 9 modified test sample.
[0027] Example 10: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 6 parts of slag powder solvent for 1-2 hours and then taken out for air drying, the air-dried recycled fine aggregate is soaked in 11 parts of water glass solvent for 1-2 hours and then taken out for air drying again, and finally the air-dried recycled fine aggregate is soaked in 6 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air drying again, thereby obtaining the modified test sample of recycled fine aggregate No. 10.
[0028] Example 11: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of slag powder solvent for 1-2 hours and then taken out for air-drying, the air-dried recycled fine aggregate is soaked in 11 parts of water glass solvent for 1-2 hours and then taken out for air-drying again, and finally the air-dried recycled fine aggregate is soaked in 11 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air-drying again, thereby obtaining the modified test sample No. 11 of recycled fine aggregate.
[0029] Example 12: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of slag powder solvent for 1-2 hours and then taken out for air drying, the air-dried recycled fine aggregate is soaked in 11 parts of water glass solvent for 1-2 hours and then taken out for air drying again, and finally the air-dried recycled fine aggregate is soaked in 6 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air drying again, thereby obtaining the modified test sample No. 12 of recycled fine aggregate.
[0030] Example 13: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of slag powder solvent for 1-2 hours and then taken out for air drying, the air-dried recycled fine aggregate is soaked in 6 parts of water glass solvent for 1-2 hours and then taken out for air drying again, and finally the air-dried recycled fine aggregate is soaked in 6 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air drying again, thereby obtaining the modified test sample No. 13 of recycled fine aggregate.
[0031] Example 14: Please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the recycled fine aggregate obtained in S1 is soaked in 11 parts of slag powder solvent for 1-2 hours and then taken out for air drying, the air-dried recycled fine aggregate is soaked in 6 parts of water glass solvent for 1-2 hours and then taken out for air drying again, and finally the air-dried recycled fine aggregate is soaked in 11 parts of polyvinyl alcohol solvent for 1-2 hours and then taken out for air drying again, thereby obtaining the modified test sample No. 14 of recycled fine aggregate.
[0032] Comparative Example 1: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as that of Example 1, except that the recycled fine aggregate is not modified by using slag powder solvent, water glass solvent or polyvinyl alcohol solvent.
[0033] Performance test 1: There are a large number of holes and gaps on the surface of the recycled fine aggregate. The presence of these holes and gaps will reduce the overall strength of the recycled aggregate and increase the water absorption rate. The water absorption rate of the recycled fine aggregate modified test samples obtained in Examples 1-14 and Comparative Example 1 and the strength of the recycled fine aggregate modified test samples were compared with the strength of natural fine aggregate; Test results: Table 1
[0034]
[0035] Furthermore, 1. by setting the slag powder solvent, the cracks and gaps on the surface of the recycled fine aggregate can be filled with the slag powder, and then the water glass solvent and the polyvinyl alcohol solvent are used to cover a thin film on the surface of the recycled fine aggregate, thereby reducing the water absorption rate of the recycled fine aggregate, thereby improving the anti-permeability and anti-freezing properties of the recycled concrete prepared with the recycled fine aggregate; 2. The more slag powder solvent participates in the modification, the higher the strength of the recycled fine aggregate modified test sample. The water glass solvent and the polyvinyl alcohol solvent can be mixed to form a gelling substance, which not only has a sticky effect, but also can fill in the cracks and gaps on the surface of the recycled fine aggregate, thereby improving the strength of the recycled fine aggregate modified test sample.
[0036] Example 15: Please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as Example 14, except that the composite fiber anti-cracking agent is made of the following raw materials: a mixture of an expander, a dispersant, a plant fiber, a polypropylene fiber and a water-retaining agent, and the mass percentages of the raw materials are: 95% expander, 1% dispersant, 1% plant fiber, 2% polypropylene raw material and 1% water-retaining agent.
[0037] Example 16, please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as Example 15, except that the composite fiber anti-cracking agent is made by mixing the following raw materials: an expander, a dispersant, a plant fiber, a polypropylene fiber and a water-retaining agent, and the mass percentages of the raw materials are: 99% expander, 0.2% dispersant, 0.2% plant fiber, 0.4% polypropylene raw material and 0.2% water-retaining agent.
[0038] Example 17, please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the composite fiber anti-cracking agent is made by mixing the following raw materials: an expander, a dispersant, a plant fiber, a polypropylene fiber and a water-retaining agent, and the mass percentages of the raw materials are: 95% expander, 1% dispersant, 1% plant fiber, 2% polypropylene raw material and 1% water-retaining agent.
[0039] Example 18, please refer to Figure 1 An embodiment provided by the present invention: The specific implementation method is the same as that of Example 1, except that the composite fiber anti-cracking agent is made by mixing the following raw materials: an expander, a dispersant, a plant fiber, a polypropylene fiber and a water-retaining agent, and the mass percentages of the raw materials are: 99% expander, 0.2% dispersant, 0.2% plant fiber, 0.4% polypropylene raw material and 0.2% water-retaining agent.
[0040] For comparative example 2, please refer to Figure 1, an embodiment provided by the present invention: the specific implementation method is the same as that of comparative example 1, except that the composite fiber anti-cracking agent is made by mixing the following raw materials: an expander, a dispersant, a plant fiber, a polypropylene fiber and a water-retaining agent, and the mass percentages of the raw materials are: 95% expander, 1% dispersant, 1% plant fiber, 2% polypropylene raw material and 1% water-retaining agent.
[0041] For comparative example 3, please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation method is the same as that of comparative example 1, except that the composite fiber anti-cracking agent is made by mixing the following raw materials: an expander, a dispersant, a plant fiber, a polypropylene fiber and a water-retaining agent, and the mass percentages of the raw materials are: 99% expander, 0.2% dispersant, 0.2% plant fiber, 0.4% polypropylene raw material and 0.2% water-retaining agent.
[0042] For comparative example 4, please refer to Figure 1 , an embodiment provided by the present invention: the specific implementation mode is the same as that of comparative example 1, except that no composite fiber anti-cracking agent is used.
[0043] Performance test 2, select the crack-resistant recycled concrete materials prepared in Examples 15-18 and Comparative Examples 2-4 to test whether there are cracks, overall compressive strength and demolition strength; Test results,Table 2
[0044] Furthermore, 1. adding a composite fiber anti-cracking agent to the recycled concrete material, the composite fiber anti-cracking agent has two anti-cracking components, namely, an expansion agent and a composite fiber, which can improve the anti-cracking ability of the recycled concrete from both physical and chemical aspects, provide double protection for the concrete, and thus significantly improve the anti-cracking performance of the recycled concrete material; 2. The expansion agent, dispersant, plant fiber, polypropylene fiber and water-retaining agent are mixed to form a composite fiber anti-cracking agent, which has the common advantages of the expansion agent and the composite fiber, can effectively solve the cracking and leakage problems of concrete engineering, and can realize the seamless construction of ultra-long structures. The prepared recycled concrete material has good compressive strength and demolition resistance, which can improve the construction efficiency and the safety of the use of recycled concrete materials.
[0045] Working principle: through the setting of slag powder solvent, the cracks and gaps on the surface of recycled fine aggregate can be filled with slag powder, and then water glass solvent and polyvinyl alcohol solvent are used to cover a thin film on the surface of recycled fine aggregate, thereby reducing the water absorption rate of recycled fine aggregate, thereby improving the anti-permeability, frost resistance and hardened strength of recycled concrete prepared with recycled fine aggregate. The more slag powder solvent participates in the modification, the higher the strength of the modified test sample of recycled fine aggregate. Water glass solvent and polyvinyl alcohol solvent can be mixed to form a gelling substance. The more they are used, the higher the strength of the modified test sample of recycled fine aggregate. Adding composite fiber anti-cracking agent to recycled concrete material In the material, the composite fiber anti-cracking agent has two anti-cracking components, namely, an expansive agent and a composite fiber, which can improve the anti-cracking ability of the recycled concrete from both physical and chemical aspects, provide double protection for the concrete, and thus significantly improve the anti-cracking performance of the recycled concrete material. The expansive agent, dispersant, plant fiber, polypropylene fiber and water-retaining agent are mixed to form a composite fiber anti-cracking agent, which has the common advantages of an expansive agent and a composite fiber, can effectively solve the cracking and leakage problems of concrete projects, and can realize the seamless construction of ultra-long structures. The prepared recycled concrete material has good compressive strength and demolition resistance, and thus can improve the construction efficiency and the safety of the use of recycled concrete materials.
[0046] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A crack-resistant recycled concrete material, characterized in that: It is made of the following raw materials in parts by weight: 18-33 parts of modifier, 33-50 parts of recycled aggregate, 37-50 parts of cement, 1-3 parts of water reducer, 8-12 parts of composite fiber anti-cracking agent, 13-23 parts of water, and 20-28 parts of sand; The modifier comprises the following raw materials in parts by weight: 6-11 parts of slag powder solvent, 6-11 parts of water glass solvent and 6-11 parts of polyvinyl alcohol solvent; The composite fiber anti-cracking agent is made of the following raw materials: expansion agent, dispersant, plant fiber, polypropylene fiber and water retaining agent, and the raw materials are mixed in the following mass percentages: expansion agent 95-99%, dispersant 0.2-1%, plant fiber 0.2-1%, polypropylene raw material 0.4-2% and water retaining agent 0.2-1%.
2. The method for preparing a crack-resistant recycled concrete material according to claim 1, characterized in that: The preparation steps of the anti-cracking recycled concrete material are as follows: S1. Grinding and crushing the recycled aggregate to obtain recycled fine aggregate; S2, soaking the recycled fine aggregate obtained in S1 in 6-11 parts of slag powder solvent for 1-2 hours, then taking it out and air-drying it, soaking the air-dried recycled fine aggregate in 6-11 parts of water glass solvent for 1-2 hours, then taking it out and air-drying it again, thereby obtaining the recycled fine aggregate No. 1 modified test sample; S3, after the plant fiber and the polypropylene fiber are evenly mixed, they are added into a twin-screw extruder for melting, extrusion, and drawing to obtain composite fibers, and then the obtained composite fibers are put into a cutting machine for crushing and cutting to obtain short-cut composite fibers; S4, mixing and stirring the chopped composite fibers obtained in S3 with the expansion agent, dispersant and water-retaining agent, and obtaining the desired composite fiber anti-cracking agent after the mixture is evenly mixed; S5, mixing the modified test sample No. 1 of recycled fine aggregate obtained in S2 with sand to obtain a mixture; S6, adding the composite fiber anti-cracking agent obtained in S4 to the preliminary mixture obtained in S5, and then mixing and stirring, and after the mixture is evenly mixed, a mixture containing the composite fiber anti-cracking agent is obtained; S7. Finally, cement, water reducing agent and water are added to the mixture with composite fiber anti-cracking agent added obtained in S5, and mixed and stirred. After being mixed evenly, the desired anti-cracking recycled concrete material is finally obtained.
3. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: The recycled fine aggregate obtained by the crushing in S1 has a particle diameter of less than 30 mm.
4. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: According to the method in S2, the same mass of recycled fine aggregate is soaked in different modifiers in turn, thereby obtaining modified test samples of various recycled fine aggregates, and the soaking time of the recycled fine aggregate in different modifiers is 1-2 hours.
5. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: In S3, the polypropylene raw material is put into a twin-screw extruder. When the twin-screw extruder is used, the extrusion temperature is 180-220° C. and the rotation speed of the twin-screw extruder is 320-400 rpm.
6. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: The polypropylene fibers obtained after melting, extrusion and drawing in S3 are put into a cutting machine for cutting to obtain short-cut polypropylene fibers with a diameter of 8-12 μm and a length of 4-9 mm.
7. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: The equipment for mixing and obtaining the composite fiber anti-cracking agent in S4 has a rotation speed of 500-750rpm and a mixing time of 45-60min, wherein the expansion agent is one of calcium oxide expansion agents, calcium sulfoaluminate expansion agents or magnesium oxide expansion agents, the dispersant is one of sodium tripolyphosphate, sodium hexametaphosphate or sodium pyrophosphate, and the water retaining agent is polyacrylamide.
8. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: The rotation speed of the modified test sample No. 1 of recycled fine aggregate in S5 when mixed with sand is 400-800 rpm, and the mixing time is 0.5-1 h.
9. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: The composite fiber anti-cracking agent in S6 is added to the preliminary mixture obtained in S5 at a mixing speed of 400-800 rpm and a mixing time of 0.5-1 h.
10. The method for preparing a crack-resistant recycled concrete material according to claim 2, characterized in that: When the desired anti-cracking recycled concrete material is obtained in S7, the mixing speed is 800-1200 rpm and the mixing time is 1-2 hours.
Citation Information
Patent Citations
Anti-seismic anti-crack mortar
CN107417210A
Regeneration asphalt concrete and preparation method thereof
CN109650824A
Composite fiber anti-cracking agent
CN113354334A