Premixed recycled aggregate pervious concrete and preparation method thereof

Through strict recycled aggregate processing, optimized mix ratio design, uniform mixing, appropriate casting and strict maintenance measures, the quality unstable and performance fluctuating of recycled aggregate concrete in the existing technology has been solved, and high strength, Highly permeable and environmentally friendly permeable concrete reduces cost and environmental impact.

CN119080449APending Publication Date: 2024-12-06YANCHENG GUOTAI CONCRETE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411298990.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the processing of existing recycled aggregates, there are problems such as unstable aggregate quality, performance fluctuations in the mixing ratio design, separation, insufficient casting density and insufficient maintenance and moisturizing insulation during the mixing process, which affects the water permeability of concrete and Durability.

Method used

Through strict regenerated aggregate processing process, optimize mix ratio design, use high-efficiency mixing equipment, adopt appropriate pouring methods and equipment, and carry out strict maintenance measures, including moisturizing and thermal insulation, to ensure the compactness and water permeability of the concrete. .

Benefits of technology

It improves the strength, durability and water permeability of concrete, reduces material costs, reduces consumption of natural resources and environmental pollution, simplifies construction difficulty, and improves construction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080449A_ABST
    Figure CN119080449A_ABST
Patent Text Reader

Abstract

The invention provides premixed recycled aggregate pervious concrete and a preparation method thereof, and relates to the technical field of concrete processing. Comprising the following components in percentage by weight: 50-70% of recycled aggregate; cement: 300 to 400 kg / m < 3 >; the water is determined according to a water-binder ratio, and the water-binder ratio is 0.45-0.55; additives: a water reducing agent, an anti-freezing agent and an anti-cracking agent, wherein the total amount does not exceed 5% of the amount of the cement; the mineral admixture comprises slag powder and fly ash, and the total amount of the mineral admixture does not exceed 30% of the use amount of the cement; the recycled aggregate is used for replacing part of natural aggregate, the material cost is reduced, by optimizing the mixing proportion and the preparation method, the strength, durability and water permeability of the concrete are improved, consumption of natural resources is reduced, environmental pollution is reduced, the mixing proportion and the preparation method are optimized, and the cost is reduced. The working performance of the concrete is improved, the construction difficulty is reduced, and the concrete has remarkable advantages in the aspects of cost, performance, environmental protection property and construction efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete processing, in particular to a premixed recycled aggregate permeable concrete and a preparation method thereof. Background Art

[0002] With the advancement of recycled aggregate technology, its performance and quality have been improved, providing a technical basis for the application of recycled aggregate in concrete. Pervious concrete technology has gradually matured, and its performance and application areas have been continuously expanded, providing technical support for the research and development of recycled aggregate pervious concrete. With the improvement of environmental awareness and the increasingly prominent urban drainage problems, the market demand for pervious concrete has continued to grow, which has promoted the research and development and application of recycled aggregate pervious concrete. Technological innovations in related fields, such as recycled aggregate processing technology, concrete mix design technology, and preparation process technology, have provided technical support for the research and development of recycled aggregate pervious concrete.

[0003] In the prior art, the processing process of recycled aggregate is relatively simple, and there may be a problem of unstable aggregate quality. The present invention ensures the stability of aggregate quality and improves the performance of concrete through a strict recycled aggregate processing process. In the prior art, the mix design mainly relies on experience, which may cause fluctuations in concrete performance. The present invention ensures the stability of concrete performance and improves durability by optimizing the mix design. In the prior art, there may be segregation in the mixing process, which affects the performance of concrete. The present invention ensures uniform mixing of concrete and avoids segregation by using efficient mixing equipment. In the prior art, there may be a problem of insufficient concrete density during the pouring process. The present invention ensures the compactness and permeability of concrete by adopting suitable pouring methods and equipment. In the prior art, there may be problems of insufficient moisture retention and heat preservation during the curing process. The present invention ensures the strength and durability of concrete through strict curing measures. Therefore, those skilled in the art provide a premixed recycled aggregate permeable concrete and a preparation method thereof to solve the problems raised in the above-mentioned background technology. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a premixed recycled aggregate permeable concrete and a preparation method thereof, which solves the problems that the existing collecting device cannot collect and store seeds well and has low screening efficiency.

[0006] (II) Technical solution

[0007] To achieve the above object, the present invention is implemented by the following technical scheme: a premixed recycled aggregate permeable concrete and a preparation method thereof, comprising the following components in weight ratio:

[0008] Recycled aggregate: 50% to 70%;

[0009] Cement: 300 to 400 kg / m 3 ;

[0010] Water: Determined by the water-to-binder ratio, which is 0.45 to 0.55;

[0011] Admixtures: water reducing agent, antifreeze agent, anti-cracking agent, the total amount shall not exceed 5% of the cement dosage;

[0012] Mineral admixtures: slag powder and fly ash, the total amount of which shall not exceed 30% of the cement dosage;

[0013] Pigments: High-performance pigments for improved color consistency;

[0014] Among them, the interconnected porosity of the recycled aggregate is greater than 15% to meet the permeability requirements of permeable concrete.

[0015] Preferably, the method comprises the following steps:

[0016] Step 1: Processing of recycled aggregate: crushing, screening and cleaning of waste concrete to obtain recycled aggregate that meets the requirements;

[0017] Step 2: Mix ratio design: Optimize the mix ratio of cement, recycled aggregate, water, admixtures and mineral admixtures according to the performance of recycled aggregate and design requirements;

[0018] Step 3: Mixing: Use efficient mixing equipment to ensure that the concrete is mixed evenly and avoid segregation;

[0019] Step 4: Pouring: Use appropriate pouring methods and equipment to ensure the compactness and permeability of the concrete;

[0020] Step 5. Curing: After pouring, proper curing, including moisture retention and heat preservation, is carried out to ensure the strength and durability of the concrete;

[0021] Step 6. Performance testing: Conduct mechanical property, durability and water permeability tests on the prepared concrete to ensure that it meets the design standards and requirements.

[0022] Preferably, the recycled aggregate is pre-treated, including crushing, screening, cleaning and surface treatment.

[0023] Preferably, the admixtures include high-efficiency water reducing agent, antifreeze agent and anti-cracking agent, and the total amount thereof does not exceed 5% of the amount of cement.

[0024] Preferably, the mineral admixtures include slag powder and fly ash, and the total amount thereof does not exceed 30% of the amount of cement.

[0025] Preferably, the pigment is a high-performance pigment used to improve the color consistency of concrete.

[0026] Preferably, the curing step includes moisturizing and heat preservation, the moisturizing temperature is 20° C. to 30° C., and the heat preservation time is 7 to 14 days.

[0027] Preferably, the performance test includes a mechanical property test, a durability test and a water permeability test.

[0028] Preferably, by optimizing the use ratio of recycled aggregate, cement dosage, water-cement ratio, use of admixtures and mineral admixtures, and the specific preparation method, the optimized premixed recycled aggregate permeable concrete of the present invention has excellent mechanical properties, durability and permeability.

[0029] Preferably, recycled aggregate is used to replace part of natural aggregate to reduce material costs.

[0030] Preferably, the strength, durability and water permeability of concrete are improved by optimizing the recycled aggregate processing, mix design, mixing, pouring and curing links.

[0031] Preferably, recycled aggregates are used to reduce the consumption of natural resources and reduce environmental pollution.

[0032] Preferably, the mix ratio and preparation method are optimized to improve the working performance of concrete and reduce the difficulty of construction.

[0033] (III) Beneficial effects

[0034] The present invention provides a premixed recycled aggregate permeable concrete and a preparation method thereof. It has the following beneficial effects:

[0035] In the present invention, recycled aggregate is used to replace part of natural aggregate, so as to reduce material cost. By optimizing the mix ratio and preparation method, the strength, durability and water permeability of concrete are improved, the consumption of natural resources is reduced, environmental pollution is reduced, the mix ratio and preparation method are optimized, the working performance of concrete is improved, and the construction difficulty is reduced. The present invention has significant advantages in cost, performance, environmental protection and construction efficiency, and has high application value and market prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the overall framework steps of the present invention;

[0037] Figure 2 It is a schematic diagram of the process of the present invention;

[0038] Figure 3 It is a schematic diagram of the raw material ratio of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Specific security risks or threats are uploaded to the risk emergency response system, which analyzes the risks or threats, blocks them through the firewall, and takes emergency repair plans and corresponding measures. At the same time, an alarm signal is sent to the control end to remind employees of the existence of security risks or threats.

[0041] Example 1: Recycled Aggregate Processing

[0042] Raw materials: waste concrete, cement, water, high-efficiency water reducing agent, antifreeze agent, anti-cracking agent, slag powder, fly ash, high-performance pigment.

[0043] Recycled Aggregate Processing:

[0044] The waste concrete is crushed to a particle size less than 10mm.

[0045] The aggregate is divided into particles of different sizes through vibration screening, and particles with a size between 5mm and 10mm are selected as recycled aggregate.

[0046] The recycled aggregate is cleaned to remove impurities and dirt.

[0047] The recycled aggregate is surface treated, such as spraying water film, to improve its bonding performance with cement. Mix design:

[0048] Proportion of recycled aggregate: Recycled aggregate accounts for 60% of the total weight of concrete.

[0049] Cement dosage: 400kg / m 3 .

[0050] Water-cement ratio: The water-cement ratio is 0.50.

[0051] Admixtures: water reducing agent, antifreeze agent, anti-cracking agent, the total amount is 5% of the cement dosage.

[0052] Mineral admixtures: slag powder, fly ash, the total amount is 30% of the cement dosage.

[0053] Pigments: High performance pigments used to improve the color consistency of concrete.

[0054] Mixing:

[0055] Mix cement, recycled aggregate, slag powder and fly ash dry materials evenly.

[0056] Add water and stir well.

[0057] Add admixture and continue stirring.

[0058] Add high performance pigment and stir well.

[0059] Casting:

[0060] Pour the mixed concrete into the mold or onto the work surface.

[0061] Use a flat plate vibrator to vibrate to ensure that the concrete is dense.

[0062] After pouring is completed, the surface is smoothed.

[0063] Maintenance:

[0064] After pouring is completed, moisturizing and heat preservation maintenance should be carried out immediately.

[0065] The curing temperature is 20℃ to 30℃.

[0066] The curing time is 7 to 14 days.

[0067] Performance Test:

[0068] Mechanical properties test: compressive strength and flexural strength tests are carried out in accordance with national standards.

[0069] Durability test: freeze-thaw cycle test, carbonization test, and impermeability test.

[0070] Water permeability test: Carry out water permeability coefficient test in accordance with national standards.

[0071] Test results:

[0072] Mechanical properties: compressive strength reaches 40MPa, flexural strength reaches 5MPa.

[0073] Durability: After 100 freeze-thaw cycle tests, there was no significant decrease in concrete strength; after 100 days of carbonization test, the carbonization depth of concrete was less than 1mm; the impermeability test reached P12 level.

[0074] Water permeability: The water permeability coefficient reaches 0.5mm / s.

[0075] in conclusion:

[0076] This example shows that by optimizing the proportion of recycled aggregate, cement dosage, water-cement ratio, use of admixtures and mineral admixtures, and the specific preparation method, the optimized premixed recycled aggregate permeable concrete of the present invention has excellent mechanical properties, durability and water permeability. The present invention has the following advantages:

[0077] Improved performance: By optimizing mix proportions and preparation methods, the strength, durability and water permeability of concrete are improved.

[0078] Reduce costs: Use recycled aggregate to replace part of natural aggregate, reducing material costs.

[0079] Enhanced environmental protection: reduced consumption of natural resources and reduced environmental pollution.

[0080] Improve construction efficiency: The optimized concrete has good working performance and improves construction efficiency.

[0081] The present invention is applicable to various permeable concrete projects, such as roads, squares, and parks, and has good application prospects.

[0082] Comparison: Cost comparison:

[0083] In the prior art, permeable concrete mainly uses natural aggregate and cement as the main raw materials. The price of natural aggregate is relatively high and the resources are limited, resulting in a high cost of permeable concrete. However, the present invention uses recycled aggregate to replace part of the natural aggregate, thereby reducing the material cost.

[0084] Existing technology: uses natural aggregate and cement, which is relatively costly.

[0085] The present invention uses recycled aggregate to replace part of natural aggregate, thereby reducing material costs.

[0086] Performance comparison:

[0087] In the prior art, the performance of permeable concrete is affected by many factors, such as aggregate quality, cement dosage, and water-binder ratio. The uncertainty of these factors leads to large fluctuations in concrete performance and insufficient durability.

[0088] Existing technology: The uncertainty of aggregate quality, cement dosage, and water-cement ratio leads to large fluctuations in concrete performance and insufficient durability.

[0089] The present invention improves the strength, durability and water permeability of concrete by optimizing the processing, mix ratio design, mixing, pouring and maintenance of recycled aggregates.

[0090] Environmental protection comparison:

[0091] In the prior art, in the production process of permeable concrete, the mining and use of natural aggregates have a certain impact on the environment. However, the present invention uses recycled aggregates, which reduces the consumption of natural resources and reduces environmental pollution.

[0092] Existing technology: The mining and use of natural aggregates have a certain impact on the environment.

[0093] The present invention uses recycled aggregates, reduces the consumption of natural resources, and reduces environmental pollution.

[0094] Construction efficiency comparison:

[0095] In the prior art, the construction process of permeable concrete is relatively complicated, requiring strict control of the mix ratio, mixing, pouring and curing links. However, the present invention improves the working performance of concrete and reduces the construction difficulty by optimizing the mix ratio and preparation method.

[0096] Existing technology: The construction process is complicated and requires strict control of the mix ratio, mixing, pouring and maintenance links.

[0097] The present invention optimizes the mix ratio and the preparation method, improves the working performance of concrete, and reduces the construction difficulty.

[0098] The following is an analysis of the specific comparison between the present invention and the prior art:

[0099] Recycled aggregate processing: In the prior art, the processing of recycled aggregate is relatively simple, and there may be problems with unstable aggregate quality. The present invention ensures stable aggregate quality and improves concrete performance through a strict recycled aggregate processing process.

[0100] Mix design: In the prior art, mix design mainly relies on experience, which may cause fluctuations in concrete performance. The present invention optimizes the mix design to ensure stable concrete performance and improve durability.

[0101] Mixing: In the prior art, segregation may occur during the mixing process, which affects the performance of concrete. The present invention ensures uniform mixing of concrete and avoids segregation by using high-efficiency mixing equipment.

[0102] Pouring: In the prior art, the concrete density may be insufficient during the pouring process. The present invention ensures the density and water permeability of the concrete by adopting a suitable pouring method and equipment.

[0103] Curing: In the prior art, the curing process may have problems of insufficient moisture retention and heat preservation. The present invention ensures the strength and durability of concrete through strict curing measures.

[0104] Compared with the prior art, the present invention has the following advantages:

[0105] Reduce costs: Use recycled aggregates to replace part of natural aggregates to reduce material costs.

[0106] Improve performance: Improve the strength, durability and water permeability of concrete by optimizing mix proportions and preparation methods.

[0107] Enhance environmental protection: reduce the consumption of natural resources and reduce environmental pollution.

[0108] Improve construction efficiency: optimize mix ratio and preparation method, improve the working performance of concrete, and reduce construction difficulty.

[0109] Therefore, the present invention has significant advantages in terms of cost, performance, environmental protection and construction efficiency, and has high application value and market prospects.

[0110] Working Principle: Firstly, select suitable waste concrete as the source of recycled aggregate to ensure its strength and cleanliness.

[0111] Crushing and screening: Crushing the waste concrete into particles smaller than 10mm, and through vibration screening, selecting particles with a size between 5mm and 10mm as recycled aggregate. This step is to remove large impurities and unqualified aggregates to ensure the particle size and quality of recycled aggregates.

[0112] Cleaning and surface treatment: Clean the recycled aggregate to remove impurities and dirt and improve its cleanliness. In addition, spray water film surface treatment technology to improve the bonding performance between recycled aggregate and cement and enhance the overall structural strength of concrete.

[0113] Mix design, recycled aggregate ratio: The optimal ratio of recycled aggregate in concrete is determined through experiments, usually around 60% to achieve a balance between cost-effectiveness and performance.

[0114] Cement dosage: Choose the appropriate amount of cement to ensure the strength and durability of the concrete.

[0115] Water-cement ratio: By precisely controlling the water-cement ratio, the fluidity and workability of the concrete can be ensured, while avoiding excessive moisture that will increase porosity and affect water permeability.

[0116] Admixtures: Use high-efficiency water reducing agent, antifreeze agent and anti-cracking agent admixtures to improve the fluidity, frost resistance and crack resistance of concrete.

[0117] Mineral admixtures: Adding slag powder and fly ash mineral admixtures not only reduces the cost but also improves the working performance and durability of concrete.

[0118] Preparation process, mixing: Use efficient mixing equipment to ensure the uniformity and consistency of concrete and avoid segregation.

[0119] Pouring: Use appropriate pouring methods and equipment to ensure the density and permeability of concrete.

[0120] Maintenance: Through moisture retention and heat preservation maintenance, ensure that the concrete is fully hardened and achieves the strength and durability required by the design.

[0121] Specific description of the working principle: Bonding action: Cement reacts chemically with recycled aggregates, mineral admixtures and admixtures to form a strong bonding structure, providing strength and durability to concrete.

[0122] Pore ​​structure: By controlling the water-cement ratio and the use of admixtures, an appropriate amount of pore structure is formed to ensure the water permeability of concrete.

[0123] Crack resistance: The use of anti-cracking agents and mineral admixtures enhances the crack resistance of concrete and improves its durability.

[0124] Antifreeze: The use of antifreeze improves the antifreeze performance of concrete in low temperature environments and prevents damage caused by freeze-thaw cycles.

[0125] Through the above working principle, this technical solution can effectively improve the performance of premixed recycled aggregate permeable concrete, so that it can meet the engineering requirements for strength, durability and permeability while maintaining economy.

[0126] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A premixed recycled aggregate permeable concrete, characterized in that: It includes the following components by weight: Recycled aggregate: 50% to 70%; Cement: 300 to 400 kg / m 3 ; Water: Determined by the water-to-binder ratio, which is 0.45 to 0.55; Admixtures: water reducing agent, antifreeze agent, anti-cracking agent, the total amount shall not exceed 5% of the cement dosage; Mineral admixtures: slag powder and fly ash, the total amount of which shall not exceed 30% of the cement dosage; Pigments: High-performance pigments for improved color consistency; Among them, the interconnected porosity of the recycled aggregate is greater than 15% to meet the permeability requirements of permeable concrete.

2. A method for preparing premixed recycled aggregate permeable concrete, characterized in that: The use of the premixed recycled aggregate permeable concrete as claimed in claim 1 comprises the following steps: Step 1: Processing of recycled aggregate: crushing, screening and cleaning of waste concrete to obtain recycled aggregate that meets the requirements; Step 2: Mix ratio design: Optimize the mix ratio of cement, recycled aggregate, water, admixtures and mineral admixtures according to the performance of recycled aggregate and design requirements; Step 3: Mixing: Use efficient mixing equipment to ensure that the concrete is mixed evenly and avoid segregation; Step 4: Pouring: Use appropriate pouring methods and equipment to ensure the compactness and permeability of the concrete; Step 5. Curing: After pouring, proper curing, including moisture retention and heat preservation, is carried out to ensure the strength and durability of the concrete; Step 6. Performance testing: Conduct mechanical property, durability and water permeability tests on the prepared concrete to ensure that it meets the design standards and requirements.

3. The method for preparing a premixed recycled aggregate permeable concrete according to claim 2, characterized in that: The recycled aggregate is pre-processed, including crushing, screening, cleaning and surface treatment.

4. The method for preparing a premixed recycled aggregate permeable concrete according to claim 2, characterized in that: The admixtures include high-efficiency water reducing agent, antifreeze agent and anti-cracking agent, and the total amount thereof does not exceed 5% of the cement dosage.

5. The method for preparing a premixed recycled aggregate permeable concrete according to claim 2, characterized in that: The mineral admixtures include slag powder and fly ash, and the total amount thereof does not exceed 30% of the cement dosage.

6. The method for preparing a premixed recycled aggregate permeable concrete according to claim 2, characterized in that: The pigments described are high performance pigments used to improve the color consistency of concrete.

7. The method for preparing a premixed recycled aggregate permeable concrete according to claim 2, characterized in that: The curing steps include moisturizing and heat preservation, the moisturizing temperature is 20° C. to 30° C., and the heat preservation time is 7 to 14 days.

8. The method for preparing a premixed recycled aggregate permeable concrete according to claim 2, characterized in that: The performance tests include mechanical performance tests, durability tests and water permeability tests.