Phosphogypsum solid waste aerated concrete and preparation method thereof

By optimizing the assembly distribution ratio and process treatment of phosphogypsum solid waste, phosphogypsum solid waste aerated concrete with high strength, stability and frost resistance was prepared, which solved the problem of phosphogypsum industrial solid waste utilization and reduced production costs and Carbon emissions meet construction application needs.

CN119080466APending Publication Date: 2024-12-06WUHAN BUILDING MATERIAL IND DESIGN & RES INST
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411181961.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively utilize phosphogypsum industrial solid waste, resulting in environmental pollution and waste of resources, and it is difficult to prepare multi-scenario and multi-purpose autoclaved aerated concrete that meets national standards.

Method used

Using the ratio of components such as cement, lime, phosphogypsum, fly ash, quartz sand tailings, composite early strength agents, bentonite, limestone powder, foaming agent and polyacrylonitrile fiber, etc., it is dried and ball milled and autoclaved. The process is used to prepare phosphogypsum solid waste aerated concrete, and use sodium carbonate and calcium sulfoaluminate cement to increase the pH value of the slurry, promote hydration reactions, and enhance the physical and mechanical properties of the product.

Benefits of technology

It significantly reduces the cost of blocks, comprehensive energy consumption and comprehensive carbon emissions, improves the strength, volume stability and frost resistance of aerated concrete, and meets the requirements of building performance and application parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080466A_ABST
    Figure CN119080466A_ABST
Patent Text Reader

Abstract

The invention provides ardealite solid waste aerated concrete and a preparation method thereof. The ardealite solid waste aerated concrete is prepared from the following components in parts by mass: 5-9 parts of cement, 10-18 parts of lime, 45-60 parts of ardealite, 9-12 parts of fly ash, 9-12 parts of quartz sand tailings, 0.8-1.2 parts of a composite early strength agent, 1-2 parts of bentonite, 0.5-1 part of limestone powder, 0.15 part of a foaming agent, 0.2-0.3 part of polyacrylonitrile fiber and 2-3 parts of wollastonite, wherein the composite early strength agent is a mixture of sodium carbonate and calcium sulphoaluminate cement. The B05-grade ardealite solid waste aerated concrete block is prepared through optimal design of a formula, 70% or above of solid waste mainly containing ardealite is utilized on the premise that the requirements for building performance, application parameters and the like are met, the cost, comprehensive energy consumption, comprehensive carbon emission and the like of the block are remarkably reduced, and the production cost is reduced. And the prepared aerated concrete block is uniform in pore structure and relatively high in closed porosity, so that the comprehensive properties such as strength, volume stability and freezing resistance of the aerated concrete are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to phosphogypsum solid waste aerated concrete and a preparation method thereof. Background Art

[0002] Aerated concrete is a porous lightweight silicate building product made of siliceous and calcareous materials as the main raw materials, mixed with gas-generating agents and other regulating materials, through processes such as batching and pouring, gas generation and static listening, cutting, autoclaving and curing (non-autoclaving). As a new type of wall building material, it has the characteristics of light weight, heat preservation, heat insulation and non-combustibility.

[0003] With the rapid development of the global economy and the urgent demand of enterprises for advanced technology, the industry has developed extremely rapidly, and the output of industrial solid waste has increased every year; a large amount of industrial solid waste is randomly piled or dumped and cannot be effectively treated, which will cause environmental pollution and waste of some resources.

[0004] Phosphogypsum is the main industrial byproduct in the process of wet preparation of phosphoric acid and production of phosphate fertilizers. It belongs to the second category of general industrial solid waste and has a gray-black or gray-white appearance. According to the survey, the production of 1 ton of phosphoric acid will produce 4-5 tons of phosphogypsum. Phosphogypsum mainly contains calcium sulfate and is highly acidic. The impurities it contains are mainly phosphate impurities, fluoride impurities, organic impurities and other impurities. Among these impurities, the phosphate and fluoride impurities have the greatest impact on the application of phosphogypsum. When phosphogypsum is used in the cement industry as a raw material or a retarder, phosphates and fluorides have a great adverse effect on cement coagulation and early compressive strength, which makes it difficult for phosphogypsum to be used on a large scale. At present, a large amount of phosphogypsum is piled up near cultivated land and rivers, which has caused serious environmental pollution problems, endangered land resources and water resources, and also had an impact on people's lives.

[0005] Therefore, how to rationally utilize construction solid waste mainly composed of phosphogypsum and reduce costs, comprehensive energy consumption, and comprehensive carbon emissions from the source, and prepare autoclaved aerated concrete that meets national standards and can be used in multiple scenarios and for multiple purposes is a technical problem that needs to be solved. Summary of the invention

[0006] The purpose of the present invention is to provide a phosphogypsum solid waste aerated concrete, which can at least solve some of the defects existing in the prior art.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] A phosphogypsum solid waste aerated concrete comprises the following components by mass: 5-9 parts of cement, 10-18 parts of lime, 45-60 parts of phosphogypsum, 9-12 parts of fly ash, 9-12 parts of quartz sand tailings, 0.8-1.2 parts of composite early strength agent, 1-2 parts of bentonite, 0.5-1 part of limestone powder, 0.15 part of foaming agent, 0.2-0.3 parts of polyacrylonitrile fiber and 2-3 parts of wollastonite; wherein the composite early strength agent is a mixture of sodium carbonate and calcium sulfoaluminate cement.

[0009] Furthermore, the mass ratio of cement to lime is 2:3-4.

[0010] Furthermore, the mass ratio of the phosphogypsum, fly ash and quartz sand tailings is 5:1:1.

[0011] Furthermore, the mass ratio of sodium carbonate and calcium sulfoaluminate cement in the composite early strength agent is 1:1.

[0012] Furthermore, the foaming agent is a composite foaming agent, which is a mixture of sodium dodecylbenzene sulfonate and aluminum powder paste in a mass ratio of 1:2.

[0013] Furthermore, the CaSO in the phosphogypsum 4 ·2H 2 The content of O is ≥65%, and the phosphogypsum is processed by ball mill after drying, and the residue passing through 200 mesh sieve is ≤10.0%.

[0014] Furthermore, the SiO 2 Content>50wt%Al 2 O 3 The content of CaCO in the limestone powder is greater than 27wt%, and the fly ash 325 mesh sieve residue is less than 12%; 3 The content of CaO in the lime is ≥ 75%, and the content of SiO in the quartz sand tailings is ≥ 100%. 2 Content ≥80%.

[0015] Furthermore, the SiO in the bentonite 2 The content is 78.3%.

[0016] Furthermore, the SiO 2 The content is ≥47wt%, and the wollastonite 200 mesh sieve residue is less than 0.4wt%; the polyacrylonitrile fiber length is 2 to 4mm.

[0017] In addition, the present invention also provides a method for preparing the above-mentioned phosphogypsum solid waste aerated concrete, comprising the following steps:

[0018] S1. Dry the phosphogypsum and process it in a ball mill, so that the residue passing through a 200-mesh sieve is ≤10.0%;

[0019] S2. Weigh cement, lime, phosphogypsum, fly ash, quartz sand tailings, composite early strength agent, bentonite, limestone powder, polyacrylonitrile fiber and wollastonite according to the designed mass ratio, add water and stir to obtain a mixed slurry, and then add the designed amount of foaming agent and stir quickly;

[0020] S3, pouring the foamed mixed slurry in step S2 into a mold, pre-curing at 45-60°C, demolding and cutting to obtain a green body, placing the green body in a steam curing autoclave for autoclaving for 6 hours, the autoclaving temperature is 180-195°C, and the pressure is 1.0-1.3MPa. After the autoclaving is completed, phosphogypsum solid waste aerated concrete is obtained.

[0021] In the present invention, the formula design principle of phosphogypsum solid waste aerated concrete is as follows:

[0022] The main raw materials such as cement, lime, quartz sand tailings, fly ash and phosphogypsum are reacted according to the prescribed mix ratios. The reaction products are mainly siliceous tobermorite, sulfur-based tobermorite, hydrated garnet, anhydrite and hydrated calcium silicate. A large amount of phosphogypsum will stimulate the reaction of silicon-calcium substances to generate hydrated calcium silicate. At the same time, sodium carbonate, calcium sulfoaluminate cement, limestone powder and the like are used as reinforcing raw materials. The added extremely fine limestone powder can serve as a crystal nucleus to promote the formation of calcium carbonate and hydrated calcium silicate products, while the calcium carbonate and a large amount of calcium sulfoaluminate generated by the rapid hydration of sodium carbonate and calcium sulfoaluminate respectively can provide a skeleton structure for the cement paste, promote the coagulation of the cement paste, and improve the early strength of the aerated concrete.

[0023] In addition, the present invention uses a large amount of phosphogypsum as the main raw material. Since the pH value of phosphogypsum is between 3 and 5, a large amount of phosphogypsum will cause the pH value of the slurry to drop from 14 to 10, ultimately affecting the normal hydration and gassing of the system, and ultimately resulting in poor physical and mechanical properties of the product. To address this problem, the present invention adds a composite early strength agent composed of sodium carbonate and calcium sulfoaluminate cement, and utilizes sodium hydroxide and aluminum hydroxide generated during the hydration reaction of sodium carbonate and calcium sulfoaluminate cement to increase the pH value of the slurry, thereby promoting the hydration reaction and ensuring the physical and mechanical properties of the product.

[0024] Fly ash can also react with CaCO in limestone powder 3Participating in the reaction, generating calcium carbonate aluminate increases the solid phase volume of the hydration product, improves the pore structure, and further improves the strength of the product. The unreacted limestone powder can also fill part of the micropores to reduce the total porosity of the product. In addition, bentonite, as an admixture, can not only adjust the performance of the slurry, but also act as an adsorbent, playing a role of bridging adsorption enhancement between the product and the raw material, so that the reaction product, the unreacted limestone powder, and part of the fly ash and quartz sand tailings that play a filling role are interconnected to form a complete whole, so that the product structure density is further enhanced, so that the solid waste can play an excellent performance. Therefore, based on the above design principle, the present invention still makes the final prepared aerated concrete have the advantages of good appearance quality, high strength, good volume stability, and good frost resistance even under the premise of a solid waste dosage of more than 70% and a short steam curing time of 6h.

[0025] A surfactant (i.e., sodium dodecylbenzene sulfonate) and aluminum powder paste are used to form a well-graded composite foam. The surfactant can reduce the surface tension of the gas-liquid interface, increase the strength and elasticity of the liquid film, rapidly reduce the pore size and pore shape factor, and enable the surface bubbles to have a double wall membrane, which can make the bubbles exist stably and increase the thickness of the bubble wall, thereby improving the physical and mechanical properties of aerated concrete.

[0026] The compounding of wollastonite and polyacrylonitrile fiber long and short makes aerated concrete outstanding in crack resistance, frost resistance and volume stability. Wollastonite, due to its fibrous morphology, can replace part of the microfibers to strengthen the cementitious material, and at the same time reduce the shrinkage and swelling rate of the product, and improve its ability to resist micro cracks caused by water loss / stress. Polyacrylonitrile fiber is an organic fiber and is used as a reinforcing fiber in the product, which has a good effect on reducing and lowering macro cracks in the product. A small amount of wollastonite and polyacrylonitrile fiber have a synergistic effect in enhancing the matrix performance and reducing micro and macro cracks, respectively. Therefore, the synergistic effect of an appropriate amount of surfactant and a small amount of wollastonite and polyacrylonitrile fiber reduces the density of aerated concrete products while improving the comprehensive properties of the products such as strength, crack resistance and frost resistance.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention prepares B05-grade phosphogypsum solid waste aerated concrete blocks through the optimized design of the formula. In terms of meeting the requirements of building performance and application parameters, more than 70% of the solid waste mainly composed of phosphogypsum is utilized, which significantly reduces the block cost, comprehensive energy consumption, comprehensive carbon emissions, etc., and the prepared phosphogypsum solid waste aerated concrete blocks have a uniform pore structure and a high closed porosity, thereby greatly improving the comprehensive properties of aerated concrete such as strength, volume stability, and frost resistance.

[0029] The present invention will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the pore structure of the phosphogypsum solid waste aerated concrete prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The present invention provides a phosphogypsum solid waste aerated concrete, comprising the following components by mass: 5-9 parts of cement, 10-18 parts of lime, 45-60 parts of phosphogypsum, 9-12 parts of fly ash, 9-12 parts of quartz sand tailings, 0.8-1.2 parts of composite early strength agent, 1-2 parts of bentonite, 0.5-1 parts of limestone powder, 0.15 parts of foaming agent, 0.2-0.3 parts of polyacrylonitrile fiber, 2-3 parts of wollastonite; wherein the composite early strength agent is a mixture of sodium carbonate and calcium sulfoaluminate cement. In addition to consuming a large amount of solid waste such as quartz sand tailings, phosphogypsum and fly ash, which account for more than 70% of the total raw materials, the prepared aerated concrete has a compressive strength of up to 5.5MPa, a density of B05 level, which is 120.0% higher than the A2.5 standard of B05-level aerated concrete, and a cost reduction of up to 21.1%, and has excellent volume stability and frost resistance.

[0033] Preferably, the mass ratio of cement to lime is 2:3-4, the mass ratio of phosphogypsum, fly ash and quartz sand tailings is 5:1:1, the mass ratio of sodium carbonate and calcium sulfoaluminate cement of the composite early strength agent is 1:1; the foaming agent is a composite foaming agent, which is a mixture of sodium dodecylbenzene sulfonate and aluminum powder paste in a mass ratio of 1:2.

[0034] Further preferably, the CaSO in the phosphogypsum 4 ·2H 2 O content ≥ 65%, and the phosphogypsum is dried and ball milled, and the residue after passing through a 200-mesh sieve is ≤ 10.0%; the SiO 2 Content>50wt%Al 2 O 3 The content of CaCO in the limestone powder is greater than 27wt%, and the fly ash 325 mesh sieve residue is less than 12%; 3 The content of CaO in the lime is ≥ 75%, and the content of SiO in the quartz sand tailings is ≥ 100%.2 Content ≥ 80%; SiO 2 The content is 78.3%; the SiO 2 The content is ≥47wt%, and the wollastonite 200 mesh sieve residue is less than 0.4wt%; the polyacrylonitrile fiber length is 2 to 4mm.

[0035] The performance of the phosphogypsum solid waste aerated concrete of the present invention is described below by means of specific examples.

[0036] Embodiment 1:

[0037] The present embodiment provides a phosphogypsum solid waste aerated concrete, including the following components by mass: 5 parts of cement, 10 parts of lime, 60 parts of phosphogypsum, 12 parts of fly ash, 12 parts of quartz sand tailings, 0.05 parts of sodium dodecylbenzene sulfonate, 0.10 parts of aluminum powder paste, 0.2 parts of polyacrylonitrile fiber, 0.8 parts of composite early strength agent (sodium carbonate: calcium sulfoaluminate cement = 1:1), 1 part of bentonite, 0.5 parts of limestone powder, and 2 parts of wollastonite.

[0038] The preparation process of phosphogypsum solid waste aerated concrete in this embodiment is as follows:

[0039] 1) After drying the phosphogypsum, it is processed in a ball mill, and the residue passing through a 200-mesh sieve is ≤10.0%.

[0040] 2) According to the above design proportion, cement, lime, quartz sand tailings, fly ash, phosphogypsum, polyacrylonitrile fiber, limestone powder, composite early strength agent, bentonite and wollastonite were weighed, water was added and mixed evenly at a stirring speed of 1200 rpm for 3 minutes to obtain a mixed slurry, and then sodium dodecylbenzene sulfonate and aluminum powder paste were poured in and stirred rapidly for 50 seconds.

[0041] 3) Pour the mixed slurry into the mold, pre-cure at 45°C for 4 hours, then demold and cut to obtain a green body of fixed specifications, place the green body in a steam curing autoclave for autoclave curing, the autoclave curing time is 6 hours, the temperature is 180°C, and the pressure is 1.0 MPa. After the autoclave curing is completed, the aerated concrete is removed from the autoclave to obtain phosphogypsum solid waste aerated concrete.

[0042] Embodiment 2:

[0043] The present embodiment provides a phosphogypsum solid waste aerated concrete, including the following components by mass: 9 parts of cement, 18 parts of lime, 45 parts of phosphogypsum, 9 parts of fly ash, 9 parts of quartz sand tailings, 0.05 parts of sodium dodecylbenzene sulfonate, 0.10 parts of aluminum powder paste, 0.3 parts of polyacrylonitrile fiber, 1.2 parts of composite early strength agent (sodium carbonate: calcium sulfoaluminate cement = 1:1), 2 parts of bentonite, 1 part of limestone powder, and 3 parts of wollastonite.

[0044] The preparation process of phosphogypsum solid waste aerated concrete in this embodiment is as follows:

[0045] 1) drying the phosphogypsum and then processing it in a ball mill, and the residue passing through a 200-mesh sieve is ≤10.0%;

[0046] 2) Cement, lime, quartz sand tailings, fly ash, phosphogypsum, polyacrylonitrile fiber, limestone powder, composite early strength agent, bentonite, and wollastonite were weighed according to the above design ratio, water was added and mixed at a stirring speed of 1200 rpm for 3 minutes to obtain a mixed slurry, and then sodium dodecylbenzene sulfonate and aluminum powder paste were poured in and quickly stirred for 50 seconds;

[0047] 3) Pour the mixed slurry into the mold, pre-cure at 60° C. for 4 h, then demold and cut to obtain a green body of fixed specifications, place the green body in a steam curing autoclave for autoclave curing, the autoclave curing time is 6 h, the temperature is 195° C., and the pressure is 1.3 MPa. After the autoclave curing is completed, the aerated concrete is removed from the autoclave to obtain phosphogypsum solid waste aerated concrete.

[0048] Embodiment 3:

[0049] The present embodiment provides a phosphogypsum solid waste aerated concrete, comprising the following components by mass: 7 parts of cement, 14 parts of lime, 50 parts of phosphogypsum, 10 parts of fly ash, 10 parts of quartz sand tailings, 0.05 parts of sodium dodecylbenzene sulfonate, 0.10 parts of aluminum powder paste, 0.3 parts of polyacrylonitrile fiber, 1.0 parts of composite early strength agent, 1.5 parts of bentonite, 0.75 parts of limestone powder, and 2 parts of wollastonite.

[0050] The preparation process of phosphogypsum solid waste aerated concrete in this embodiment is as follows:

[0051] 1) After drying the phosphogypsum, it is processed in a ball mill, and the residue passing through a 200-mesh sieve is ≤10.0%.

[0052] 2) According to the above design proportion, cement, lime, quartz sand tailings, fly ash, phosphogypsum, polyacrylonitrile fiber, limestone powder, composite early strength agent, bentonite and wollastonite were weighed, water was added and mixed evenly at a stirring speed of 1200 rpm for 3 minutes to obtain a mixed slurry, and then sodium dodecylbenzene sulfonate and aluminum powder paste were poured in and stirred rapidly for 50 seconds.

[0053] 3) Pour the mixed slurry into the mold, pre-cure at 55° C. for 4 hours, then demold and cut to obtain a green body of fixed specifications, place the green body in a steam curing autoclave for autoclave curing, the autoclave curing time is 6 hours, the temperature is 190° C., and the pressure is 1.2 MPa. After the autoclave curing is completed, the aerated concrete is removed from the autoclave to obtain phosphogypsum solid waste aerated concrete.

[0054] Embodiment 4:

[0055] The present embodiment provides a phosphogypsum solid waste aerated concrete, including the following components in parts by mass: 8 parts of cement, 12 parts of lime, 50 parts of phosphogypsum, 10 parts of fly ash, 10 parts of quartz sand tailings, 0.05 parts of sodium dodecylbenzene sulfonate, 0.10 parts of aluminum powder paste, 0.25 parts of polyacrylonitrile fiber, 1.1 parts of composite early strength agent, 1 part of bentonite, 0.8 parts of limestone powder, and 2 parts of wollastonite.

[0056] The preparation process of phosphogypsum solid waste aerated concrete in this embodiment is as follows:

[0057] 1) After drying the phosphogypsum, it is processed in a ball mill, and the residue passing through a 200-mesh sieve is ≤10.0%.

[0058] 2) Cement, lime, quartz sand tailings, fly ash, phosphogypsum, polyacrylonitrile fiber, limestone powder, composite early strength agent, bentonite, and wollastonite were weighed according to the above design ratio, water was added and mixed at a stirring speed of 1200 rpm for 3 minutes to obtain a mixed slurry, and then sodium dodecylbenzene sulfonate and aluminum powder paste were poured in and quickly stirred for 50 seconds;

[0059] 3) Pour the mixed slurry into the mold, pre-cure at 60° C. for 4 h, then demold and cut to obtain a green body of fixed specifications, place the green body in a steam curing autoclave for autoclave curing, the autoclave curing time is 6 h, the temperature is 195° C., and the pressure is 1.3 MPa. After the autoclave curing is completed, the aerated concrete is removed from the autoclave to obtain phosphogypsum solid waste aerated concrete.

[0060] Comparative Example:

[0061] This comparative example uses conventional aerated concrete, which includes the following components by mass: 9 parts of cement, 18 parts of lime, 70 parts of quartz sand tailings, 3 parts of desulfurized gypsum, and 0.10 parts of aluminum powder paste.

[0062] The preparation process of aerated concrete is as follows:

[0063] 1) Weigh cement, lime, quartz sand tailings, desulfurized gypsum, and aluminum paste according to the designed proportion, add water and mix evenly at a stirring speed of 1200 rpm to obtain a mixed slurry;

[0064] 2) Pour the mixed slurry into the mold, pre-cure at 60°C for 4 hours, then demould and cut to obtain a green body of fixed specifications, place the green body in a steam curing autoclave for autoclave curing, the autoclave curing time is 8 hours, the temperature is 195°C, and the pressure is 1.3 MPa. After the autoclave curing is completed, the aerated concrete is removed from the autoclave to obtain the aerated concrete.

[0065] The physical and mechanical properties and costs of the above-mentioned Examples 1 to 4 and the comparative example are compared, and the results are shown in Table 1.

[0066] Table 1:

[0067] Detection indicators Example 1 Example 2 Example 3 Example 4 Comparative Example Density level B05 B05 B05 B05 B05 Compressive strength(MPa) 4.70 5.50 5.18 5.02 3.51 Freezing resistance-mass loss (%) 0.89 0.55 0.68 0.77 4.30 Frost resistance-strength loss (%) 9.77 7.02 8.11 9.39 17.02 <![CDATA[Cost (yuan / m 3 )]]> 150.37 165.76 158.99 156.13 190.49

[0068] It can be seen from the aerated concrete test results in Table 1 that among the aerated concrete prepared by the same molding process, the aerated concrete prepared by the present invention has high compressive strength, low cost, low comprehensive energy consumption, and low comprehensive carbon emissions. At the same time, its frost resistance and weather resistance experiments show that the aerated concrete of the present invention still guarantees the integrity of the aerated concrete after 15 freeze-thaw cycles. The mass loss rate after 15 freeze-thaw cycles is only 0.55-0.89%, and the compressive strength loss rate is only 7.02-9.77%. The cost is reduced by up to 21.1%, and the physical and mechanical properties are much higher than the requirements of aerated concrete in GB / T11969-2020. The aerated concrete in the comparative example is a common aerated concrete formula with low compressive strength, high cost, high comprehensive energy consumption, large comprehensive carbon emissions, and poor frost resistance and weather resistance, which can only barely meet the requirements of national standards B05 and A3.5. Therefore, the aerated concrete blocks of the present invention significantly reduce the block cost, comprehensive energy consumption, comprehensive carbon emissions, etc. in terms of meeting the requirements of building performance and application parameters, greatly improve the comprehensive performance of aerated concrete such as strength, volume stability, frost resistance, etc., and significantly enhance the core competitiveness of the product.

[0069] Embodiment 5:

[0070] Effect of the ratio of cement to lime on the performance of aerated concrete in this embodiment. In order to reflect the difference in the effect of the ratio of cement to lime on the performance of aerated concrete, this embodiment designed five groups of experiments, namely, Group A, Group B, Group C, Group D, and Group E, for comparison, wherein Group A adopted the formula of the above-mentioned embodiment 2, Group B contained 6 parts of cement and 9 parts of lime, and the remaining components were the same as those of Group A, Group C contained 8 parts of cement and 14 parts of lime, and the remaining components were the same as those of Group A, Group D contained 11 parts of cement and 11 parts of lime, and the remaining components were the same as those of Group A, and Group E contained 8 parts of cement and 20 parts of lime, and the remaining components were the same as those of Group A. The aerated concrete preparation processes of Group A, Group B, Group C, Group D, and Group E in this embodiment were consistent, all the same as those in the above-mentioned embodiment 2. The physical and mechanical properties of the aerated concrete obtained from Group A, Group B, Group C, Group D, and Group E in this embodiment were tested, and the results are shown in Table 2.

[0071] Table 2:

[0072] Detection indicators A B C D E Density level B05 B05 B05 B05 B06 Compressive strength(MPa) 5.50 5.13 5.32 3.84 3.47 Freezing resistance-mass loss (%) 0.55 0.78 0.66 2.99 3.68 Frost resistance-strength loss (%) 7.02 8.15 7.59 11.27 12.32

[0073] It can be seen from the aerated concrete test results in Table 2 that in the aerated concrete prepared by the same molding process, the ratio of cement to quicklime in groups A, B, and C is 2:3-4, and the obtained aerated concrete has high compressive strength. At the same time, its frost resistance and weather resistance experiment shows that the aerated concrete of the present invention still guarantees the integrity of the aerated concrete after 15 freeze-thaw cycles, and the mass loss rate after 15 freeze-thaw cycles is only 0.55-0.78%, and the compressive strength loss rate is only 7.02-8.15%. The physical and mechanical properties are much higher than the requirements of aerated concrete in GB / T11969-2020; and the aerated concrete of groups D and E has low compressive strength and poor frost resistance and weather resistance because the ratio of cement to quicklime is 1:1 and 2:5, respectively. Therefore, the ratio of cement to quicklime plays a vital role in the performance of aerated concrete blocks. Too high or too low a ratio of cement to quicklime will reduce the compressive strength and frost resistance of the aerated concrete.

[0074] Embodiment 6:

[0075] This example investigates the effects of phosphogypsum, fly ash and quartz sand tailings on the performance of the prepared aerated concrete. In order to reflect the differences in the effects of phosphogypsum, fly ash and quartz sand tailings on the performance of aerated concrete, this example designs 7 groups of experiments, including Group A, Group B, Group C, Group D, Group E, Group F and Group G, for comparison, wherein Group A adopts the formula of the above-mentioned Example 2, Group B contains 0 fly ash components, Group C contains 0 quartz sand tailings components, Group D contains 0 phosphogypsum components, Group E contains 54 phosphogypsum components, Group F contains 18 fly ash components, Group G contains 6 fly ash components, and the remaining components in each group are the same as Group A. The aerated concrete preparation process of all groups in this example is consistent, all the same as the above-mentioned Example 2. The physical and mechanical properties of the aerated concrete prepared by all groups in this example are tested, and the results are shown in Table 3.

[0076] Table 3:

[0077] Detection indicators A B C D E F F Density level B05 B05 B05 B05 B05 B05 B05 Compressive strength(MPa) 5.50 3.21 3.44 3.89 3.77 3.15 3.07 Freezing resistance-mass loss (%) 0.55 3.79 3.58 2.91 3.55 3.82 3.95 Frost resistance-strength loss (%) 7.02 12.15 12.27 12.55 11.98 12.06 13.22

[0078] It can be seen from the aerated concrete test results in Table 3 that among the aerated concrete prepared by the same molding process, the compressive strength of the aerated concrete prepared in group A can reach up to 5.50 MPa. At the same time, its frost resistance and weather resistance experiment shows that the aerated concrete of the present invention still guarantees the integrity of the aerated concrete after 15 freeze-thaw cycles. The mass loss rate after 15 freeze-thaw cycles is only 0.55%, and the compressive strength loss rate is only 7.02%. The physical and mechanical properties are much higher than the requirements of aerated concrete in GB / T11969-2020; while the aerated concrete of the other 6 groups did not add phosphogypsum, fly ash and quartz sand tailings at the same time or did not follow the method of the present invention. The above materials are added in a certain proportion, and the compressive strength is low and the frost resistance and weather resistance are poor. The main reasons are: a large amount of phosphogypsum will stimulate the reaction of silicon-calcium substances to generate hydrated calcium silicate. In addition, calcium sulfate in phosphogypsum can participate in the reaction to generate calcium alumina to improve the early strength. Later, under steam curing conditions, tobermorite, water garnet and other reaction products are generated to improve the performance; quartz sand tailings mainly play the role of inert aggregate, and can react with calcium hydroxide to generate hydrated calcium silicate and tobermorite under steam curing conditions; fly ash is a volcanic ash material, which can undergo hydration reaction at room temperature to improve the early strength, and the active alumina in fly ash can also react with CaCO in limestone powder to form hydrated calcium silicate and tobermorite. 3 The participation in the reaction to generate calcium carbonoaluminate increases the solid volume of the hydration product, improves the pore structure, and further increases the strength of the product. The synergistic effect of the three in the set ratio has a significant enhancement effect on the performance of aerated concrete blocks.

[0079] Embodiment 7:

[0080] This embodiment investigates the effects of composite early strength agent, bentonite and limestone powder on the performance of the prepared aerated concrete. In order to reflect the difference in the effects of composite early strength agent, bentonite and limestone powder on the performance of aerated concrete, this embodiment designs eight groups of experiments, namely, Group A, Group B, Group C, Group D, Group E, Group F, Group G and Group H, for comparison, wherein Group A adopts the formula of the above-mentioned embodiment 2, Group B contains 0 components of composite early strength agent, Group C contains 0 components of bentonite, Group D contains 0 components of limestone powder, Group E contains 0 components of composite early strength agent and bentonite, Group F contains 0 components of bentonite and limestone powder, Group G contains 0 components of composite early strength agent and limestone powder, Group H contains 0 components of composite early strength agent, bentonite and limestone powder, and the remaining components in each group are the same as those in Group A. The aerated concrete preparation process of all groups in this embodiment is consistent, all the same as in the above-mentioned embodiment 2. The physical and mechanical properties of the aerated concrete obtained by all groups in this embodiment are tested, and the results are shown in Tables 4 and 5, respectively.

[0081] Table 4:

[0082] Detection indicators A B C D Density level B05 B05 B05 B05 Compressive strength(MPa) 5.50 4.01 4.16 4.18 Freezing resistance-mass loss (%) 0.55 2.08 2.01 2.03 Frost resistance-strength loss (%) 7.02 9.55 9.35 9.46

[0083] Table 5:

[0084] Detection indicators E F G H Density level B05 B05 B05 B05 Compressive strength(MPa) 3.23 3.89 3.29 2.96 Freezing resistance-mass loss (%) 3.14 3.08 3.22 4.11 Frost resistance-strength loss (%) 10.78 10.01 10.91 16.84

[0085] It can be seen from the aerated concrete test results in Tables 4 and 5 that among the aerated concrete prepared by the same molding process, the compressive strength of the aerated concrete prepared in Group A can reach up to 5.50 MPa. At the same time, its frost resistance and weather resistance experiments show that the aerated concrete of the present invention still guarantees the integrity of the aerated concrete after 15 freeze-thaw cycles. The mass loss rate after 15 freeze-thaw cycles is only 0.55%, and the compressive strength loss rate is only 7.02%. The physical and mechanical properties are much higher than the requirements of aerated concrete in GB / T11969-2020; while the aerated concrete of the other 7 groups has low compressive strength and poor frost resistance and weather resistance because the composite early strength agent, bentonite and limestone powder are not added at the same time. The main reason is that the added extremely fine limestone powder can act as a crystal nucleus to promote the formation of calcium carbonate and calcium silicate hydrate products, and sodium carbonate and calcium sulfoaluminate are quickly hydrated. The calcium carbonate and a large amount of calcium sulfonate generated by chemical reaction can provide a skeleton structure for the cement paste, promote the coagulation of the cement paste, and improve the early strength of the aerated concrete. Since the pH value of phosphogypsum is between 3 and 5, a large amount of phosphogypsum will cause the pH value of the slurry to drop from 14 to 10, which will eventually affect the hydration and gasification of the system. However, the sodium hydroxide and aluminum hydroxide generated by the composite early strength agent during the hydration reaction can increase the pH value of the slurry and promote the hydration reaction. In addition, bentonite plays a bridging adsorption role between the product and the raw materials, so that the reaction product, the unreacted limestone powder, and some of the fly ash and quartz sand tailings that play a filling role are interconnected to form a complete whole, and the structural density is further enhanced, so that the solid waste can play an excellent performance; bentonite is used as an admixture to adjust the performance of the slurry and as an adsorbent, it plays a bridging adsorption enhancement effect.

[0086] The above examples are merely illustrative of the present invention and do not constitute a limitation on the protection scope of the present invention. All designs that are the same or similar to the present invention fall within the protection scope of the present invention.

Claims

1. A phosphogypsum solid waste aerated concrete, characterized in that: The invention comprises the following components by mass: 5-9 parts of cement, 10-18 parts of lime, 45-60 parts of phosphogypsum, 9-12 parts of fly ash, 9-12 parts of quartz sand tailings, 0.8-1.2 parts of composite early strength agent, 1-2 parts of bentonite, 0.5-1 parts of limestone powder, 0.15 parts of foaming agent, 0.2-0.3 parts of polyacrylonitrile fiber and 2-3 parts of wollastonite; wherein the composite early strength agent is a mixture of sodium carbonate and calcium sulfoaluminate cement.

2. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The mass ratio of cement to lime is 2:3-4.

3. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The mass ratio of the phosphogypsum, fly ash and quartz sand tailings is 5:1:

1.

4. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The mass ratio of sodium carbonate and calcium sulphoaluminate cement in the composite early strength agent is 1:

1.

5. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The foaming agent is a composite foaming agent, which is a mixture of sodium dodecylbenzene sulfonate and aluminum powder paste in a mass ratio of 1:

2.

6. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The content of CaSO4·2H2O in the phosphogypsum is ≥65%, and the phosphogypsum is dried and ball milled, and the residue passing through a 200-mesh sieve is ≤10.0%.

7. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The SiO2 content in the fly ash is greater than 50wt%, the Al2O3 content is greater than 27wt%, and the fly ash 325 mesh sieve residue is less than 12%; the CaCO3 content in the limestone powder is greater than 98wt%, and the limestone powder 1500 mesh sieve residue is less than 1wt%; the CaO content in the lime is ≥75%, and the SiO2 content in the quartz sand tailings is ≥80%.

8. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The SiO2 content in the bentonite is 78.3%.

9. The phosphogypsum solid waste aerated concrete according to claim 1, characterized in that: The content of SiO2 in the wollastonite is ≥47wt%, and the residue on a 200-mesh sieve of the wollastonite is less than 0.4wt%; the length of the polyacrylonitrile fiber is 2-4mm.

10. The method for preparing phosphogypsum solid waste aerated concrete according to any one of claims 1 to 9, characterized in that: The steps include: S1, drying the phosphogypsum and then processing it in a ball mill, so that the residue passing through a 200-mesh sieve is ≤10.0%; S2. Weigh cement, lime, phosphogypsum, fly ash, quartz sand tailings, composite early strength agent, bentonite, limestone powder, polyacrylonitrile fiber and wollastonite according to the designed mass ratio, add water and stir to obtain a mixed slurry, and then add the designed amount of foaming agent and stir quickly; S3, pouring the foamed mixed slurry in step S2 into a mold, pre-curing at 45-60°C, demolding and cutting to obtain a green body, placing the green body in a steam curing autoclave for autoclaving for 6 hours, the autoclaving temperature is 180-195°C, and the pressure is 1.0-1.3MPa. After the autoclaving is completed, phosphogypsum solid waste aerated concrete is obtained.

Citation Information

Cited By

  • Aerated concrete product based on tail mud with high methylene blue value and preparation method of aerated concrete product

    CN120398504A

  • Aerated concrete products based on high methylene blue value tailings and their preparation methods

    CN120398504B