Method for producing sintered blue corundum
During the sintering process of blue corundum, the uniform mixing of high-purity alumina powder and titanium blue and temperature curve control technology are used to solve the crack problem during the sintering process of blue corundum, which improves the consistency and stability of the product and ensures high quality finished product.
Patent Information
- Application Number
- CN202411198229.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
During the sintering of blue corundum, crack problems caused by thermal stress and uneven shrinkage affect the product yield and quality.
By mixing high-purity alumina powder with titanium blue to form raw material powder and forming under preset pressure conditions, combined with sintering technology controlled by temperature curve, reduce internal stress, ensure uniform temperature rise and fall, reduce the risk of thermal deformation, and Cool naturally during cooling to avoid cracks caused by rapid cooling.
It effectively reduces the possibility of cracks and damage of the product, improves the consistency and stability of blue corundum materials, ensures the quality reliability of the product, and significantly improves the integrity and aesthetics of the product.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sintering inorganic non-metallic materials, in particular to a method for producing sintered blue corundum. Background Art
[0002] Blue corundum is a gem-quality variety of corundum known for its deep blue color. Corundum is a mineral whose chemical composition is primarily aluminum oxide. Blue corundum is one of the most well-known varieties of corundum and is often used in jewelry for its beautiful color and hardness. Blue corundum is generally produced by sintering, a process in which blue corundum powder is heated under high temperature conditions to form a solid material.
[0003] In this process, in order to improve the blue corundum grain structure, an appropriate amount of stabilizer or promoter is added. However, due to factors such as thermal stress and uneven shrinkage during the sintering process, cracks often appear in blue corundum products, which has a significant impact on the yield and quality of the final product. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a method for producing sintered blue corundum, which solves the common product cracking problem in traditional production methods.
[0005] To achieve the above object, the present invention is implemented by the following technical scheme: a method for producing sintered blue corundum, comprising the following steps:
[0006] S1. A raw material powder is formed by mixing high-purity alumina powder and titanium blue;
[0007] S2. molding the raw material powder under a predetermined pressure to obtain a green body;
[0008] S3. Controlling the heating rate in the sintering furnace based on the temperature curve to reduce internal stress;
[0009] S4. Cool the sintered blue corundum and remove surface defects of the product.
[0010] Preferably, the S1 step is specifically as follows:
[0011] Weigh high-purity alumina powder according to the mass ratio;
[0012] Add titanium blue to pre-treated high-purity alumina powder;
[0013] The mixture is uniformly mixed using a ball mill;
[0014] Remove large particles generated during the mixing process by sieving;
[0015] The processed powder is placed in a stirring device to further improve the mixing degree to obtain a raw material powder.
[0016] Preferably, the S2 step is specifically as follows:
[0017] Placing the prepared raw material powder in a compression mold;
[0018] Density is ensured by adjusting the pressure of the die press to a predetermined tonnage range;
[0019] Control the speed of the pressurization process to ensure uniform material distribution;
[0020] After the pressing is completed, it is held for a short time to stabilize the structure and then the pressing die is released;
[0021] The formed green embryo is demoulded and set aside.
[0022] Preferably, the S3 step is specifically as follows:
[0023] Set the temperature gradient within the sintering program according to material properties;
[0024] The material box loaded with green compacts is sent into a sintering furnace that has been preheated to a specified temperature range, and preheated at the preheating temperature for 5 minutes;
[0025] Execute the step-by-step increase of the heating rate within the lower and upper limits of the set temperature curve until the maximum heating rate R_max is reached, and keep the rate unchanged within the set time T_i nter. When the temperature in the sintering furnace reaches the preset maximum temperature, adjust the heating rate to ensure that the temperature of each part rises evenly and reduce the risk of thermal deformation;
[0026] Monitor changes in the furnace environment to ensure that they do not exceed safety limits;
[0027] After keeping the temperature for a certain period of time until the material crystal phase transformation is completed or the pores are completely eliminated, continue to maintain it for a period of time until the internal microstructure is stable to complete solid phase sintering.
[0028] Preferably, the S4 step is specifically as follows:
[0029] Slowly lower the furnace temperature to a point where it can be safely removed from the furnace without damaging the product;
[0030] Remove the product crystal and place it in an air convection environment for natural cooling to avoid cracks caused by rapid cooling;
[0031] Clean the sticky residue on the outside of the product to reveal the original color and shape of the product and observe whether the surface is flat and has no obvious defects;
[0032] If there is a rough surface or pore defect, use tools to gently grind it until the surface is bright, smooth and without cracks;
[0033] After confirming that surface defects have been removed, a final quality inspection is carried out to ensure the pass rate and prepare for subsequent processing or storage.
[0034] Preferably, when gradually increasing the heating rate until reaching the maximum heating rate R_max, it specifically includes:
[0035] If the current heating rate R < R_max, then increase the actual heating rate R by 1 degree Celsius per minute;
[0036] Continue to adjust when the heating speed is less than the difference between the maximum heating speed and the target heating speed;
[0037] Detect whether the difference between the real-time temperature T_real and the heating curve T_ideal under ideal conditions exceeds the allowable deviation △T. When it exceeds △T, fine-tune the heating rate;
[0038] Dynamically correct the deviation during the heating process based on the information fed back by the temperature control system.
[0039] Preferably, dynamically correct the deviation during the heating process based on the information fed back by the temperature control system, specifically including:
[0040] Calculate the square of the difference between the actual temperature change rate V and the set ideal temperature change rate V_ideal, that is, △V^2 = (V - V_ideal)^2;
[0041] When △V^2 > the preset correction condition, execute the rate correction process, and at the same time monitor whether it exceeds the maximum allowable temperature deviation limit of ±3°C;
[0042] After adjustment, recalculate △V^2, and repeat the above until the heating is stable or a new correction condition is reached;
[0043] Determine the next action of the heating control strategy based on the satisfaction of the correction condition.
[0044] Preferably, repeat the above until the heating is stable or a new correction condition is reached, specifically including:
[0045] Detect whether the decrease amplitude of △V decreases continuously three times. If it decreases, it means gradually stable and stop the correction program;
[0046] Judge whether the heating duration t reaches the specified total heating duration T. When t ≥ T, it means reaching the end stage of the heating process;
[0047] During the constant temperature holding time, if the fluctuation amplitude ΔT > ±2°C appears, it is necessary to resume the correction cycle until ΔT ≤ ±0.2°C.
[0048] The present invention provides a method for producing sintered blue corundum. It has the following beneficial effects:
[0049] 1. The present invention ensures the quality and structure of subsequent products by pressing the prepared raw material powder into a green body of a specific shape under preset pressure conditions; the obtained green body is placed in a sintering furnace with pre-adjusted heating parameters such as heating and cooling rates, and sintering treatment is performed based on a temperature change curve under precise control. The temperature curve design in this process is a key innovation point, which can effectively reduce the thermal stress caused by thermal expansion inside the product during the heating and cooling stages, thereby greatly reducing the possibility of defects such as cracks and breakages in the product, improving the consistency and stability of the blue corundum material, solving the problem of product cracking common in traditional production methods, and ensuring the quality reliability of blue corundum products. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0051] Example:
[0052] The embodiment of the present invention provides a method for producing sintered blue corundum, comprising the following steps:
[0053] S1. Weigh high-purity alumina powder according to the mass ratio, add titanium blue to the pre-treated high-purity alumina powder, and use a ball mill to continuously mix the mixture for 20-40 hours until a dark blue mixture with uniform color and no particles is obtained. Remove large particles generated during the mixing process through sieving, and place the treated powder into a stirring device to further improve the mixing degree to obtain a raw material powder.
[0054] S2. Place the prepared raw material powder in a die, and use a die pressing machine to pressurize the prepared raw material powder in a customized metal mold under a pressure condition of 5 to 20 MPa for two to three minutes. During the process of applying the compressive force, ensure that the action is smooth and even rather than increasing suddenly, so that the powder material can be subjected to basically consistent effective pressure in the entire mold area. While completing the pressing action, continue to keep the blank in the same pressure environment for a period of time without stress change to enhance the stability of its internal organizational structure and eliminate excess bubble substances. Demold the formed blank for use.
[0055] S3. Set the heating rate gradient in the sintering process according to the material properties. The heating rate gradient includes the maximum temperature (1550 °C to 1650 °C), the heating rate (between 5 °C / min and 10 °C / min), the holding time (1 to 4 hours), and the cooling rate (5 °C / min to 10 °C / min). Send the cartridge loaded with green compacts into the sintering furnace that has been preheated to the specified temperature range, and preheat it at a preheating temperature of 900 °C for 5 minutes; gradually increase the heating rate until the maximum heating rate R_max is reached, and keep this rate unchanged within the set time T_inter. When the temperature in the sintering furnace reaches the preset maximum temperature, adjust the heating rate to ensure that the temperature of each part rises evenly and reduce the risk of thermal deformation; monitor the changes in the furnace environment to ensure that it does not exceed the safety limit. After holding for a certain time until the temperature at which the material phase transformation is completed or the pores are completely removed, continue to maintain for a period of time until the internal microstructure is stable to complete solid-phase welding.
[0056] S4. Slowly lower the temperature of the heated furnace body until it reaches below 200 °C, and place the product cooled to a safe temperature in a natural convection ventilation environment at room temperature for further cooling; clean the adhesion residues on the outside of the product to expose the original color and shape of the product and observe whether the surface is flat and has obvious defects; if there are rough or uneven surfaces or pore defects, gently grind them with tools until the surface is bright, smooth and free of cracks; after confirming the removal of surface defects, conduct a final quality inspection to ensure the qualified rate and prepare for subsequent processing or storage in the warehouse.
[0057] The above-mentioned gradually increasing the heating rate until the maximum heating rate R_max is reached specifically includes:
[0058] If the current heating rate R < R_max, then increase the actual heating rate R by 1 °C / min;
[0059] Continue to adjust when the heating speed is less than the difference between the maximum heating speed and the target heating speed;
[0060] Detect whether the difference between the real-time temperature T_real and the heating curve T_ideal under ideal conditions exceeds the allowable deviation △T, and fine-tune the heating rate when it exceeds △T;
[0061] Dynamically correct the deviation in the heating process based on the information fed back by the temperature control system.
[0062] The above-mentioned dynamically correcting the deviation in the heating process based on the information fed back by the temperature control system specifically includes:
[0063] Calculate the square of the difference between the actual temperature change rate V and the set ideal temperature change rate V_ideal, that is, △V^2 = (V - V_ideal)^2;
[0064] When △V^2>preset correction condition, the rate correction process is executed, and at the same time, it is monitored whether it exceeds the maximum allowable temperature deviation limit of ±3℃;
[0065] Recalculate △V^2 after adjustment, and repeat the above steps until the heating is stable or the new correction conditions are reached;
[0066] The next action of the heating control strategy is determined based on the satisfaction of the correction conditions.
[0067] Repeat the above until the heating is stable or reaches a new correction condition, including:
[0068] Check whether the reduction of △V decreases three times in a row. If it decreases, it means that it is gradually stabilizing and the correction procedure is stopped;
[0069] Determine whether the heating duration t reaches the specified total heating duration T. When t ≥ T, it indicates that the heating process has reached the end stage;
[0070] If the fluctuation range ΔT>±2℃ appears during the constant temperature holding time, it is necessary to restore the correction cycle until ΔT≤±0.2℃.
[0071] In summary, the present invention firstly forms the required raw material powder by accurately mixing high-purity alumina powder with titanium blue, and this step is to ensure the color and material consistency of the final product; secondly, the prepared raw material powder is pressed into a green body of a specific form under preset pressure conditions to ensure the quality and structure of subsequent products; the third step is to put the obtained green body into a sintering furnace with pre-adjusted heating parameters such as heating and cooling rates, and sintering treatment is carried out based on the temperature change curve under precise control. The temperature curve design in this process is the key innovation point, which can effectively reduce the thermal stress caused by thermal expansion inside the product during the heating and cooling stages, thereby greatly reducing the possibility of cracks, breakage and other defects in the product, improving the consistency and stability of the blue corundum material, solving the common problems of product cracking in traditional production methods, and ensuring the quality reliability of blue corundum products; finally, the blue corundum product that has completed the sintering process is gradually cooled to room temperature, and various possible adverse factors on the surface of the finished product after cooling are removed as necessary. In this way, a blue corundum product with excellent quality can be obtained.
[0072] This process can not only significantly improve the integrity of the product, but also improve the quality and aesthetics of the final product, which has a positive effect on the expansion of the application field of blue corundum. By refining and optimizing each step, this process provides reliable process support and guarantee for the industrial mass production of high-quality, low-loss blue corundum products. Its most prominent feature is that it can overcome the cracking problem that is often encountered and difficult to cure in the previous processing process, so that the mechanical processing properties, wear resistance and decorative aesthetics of the finished product can be comprehensively improved.
[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for producing sintered blue corundum, characterized in that: It includes the following steps: S1. Form a raw material powder by mixing high-purity alumina powder and titanium blue. S2. Mold the raw material powder under a predetermined pressure to obtain a green body. S3. Control the heating rate in the sintering furnace based on the temperature curve to reduce internal stress. S4. Cool the sintered sapphire and remove the defects on the surface of the product.
2. A method for producing sintered blue corundum according to claim 1, characterized in that: The specific steps of S1 are as follows: Weigh the high-purity alumina powder according to the mass ratio. Add titanium blue to the pre-treated high-purity alumina powder. Use a ball mill to uniformly mix the mixture. Remove the large particle substances generated during the mixing process through sieving. Put the treated powder into a stirring device to further improve the mixing degree to obtain the raw material powder.
3. A method for producing sintered blue corundum according to claim 1, characterized in that: The specific steps of S2 are as follows: Place the prepared raw material powder in a mold. Ensure the density by adjusting the pressure of the molding machine to a predetermined tonnage range. Control the speed of the pressing process to make the material distribution uniform. After pressing, hold for a short time to stabilize the structure and release the mold. Demold the molded green body and set it aside for later use.
4. A method for producing sintered blue corundum according to claim 1, characterized in that: The specific steps of S3 are as follows: Set the heating gradient in the sintering program according to the material characteristics. Send the cartridge loaded with the green body into the sintering furnace that has been preheated to the specified temperature range, and preheat at the preheating temperature for 5 minutes. Execute a step-by-step increase in the heating rate within the lower and upper limit ranges of the set temperature curve until the maximum heating rate R_max is reached, and maintain this rate unchanged within the set time T_inter. When the temperature in the sintering furnace reaches the preset maximum temperature, adjust the heating rate to ensure that the temperature of each part rises evenly and reduce the risk of thermal deformation. Monitor the changes in the furnace environment to ensure that it does not exceed the safety limit. Keep the temperature for a certain period of time until the temperature at which the material phase transformation is completed or the pores are completely removed, and then continue to maintain for a period of time until the internal microstructure is stable to complete the solid-phase welding.
5. A method for producing sintered blue corundum according to claim 1, characterized in that: The specific steps of S4 are as follows: Slowly reduce the furnace temperature until it reaches a temperature at which it can be safely removed from the furnace without damaging the product. Take out the product and place it in an air convection environment to cool naturally to avoid cracks caused by rapid cooling. Clean the adhesion residues on the outside of the product to expose the original color and shape of the product and observe whether the surface is flat and has obvious defects. If there are rough or uneven surfaces or pore defects, gently grind them with tools until the surface is smooth and shiny without cracks. After confirming the removal of surface defects, conduct a final quality inspection to ensure the qualified rate and prepare for subsequent processing or storage in the warehouse.
6. A method for producing sintered blue corundum according to claim 5, characterized in that: When gradually increasing the heating rate until the maximum heating rate R_max is reached, it specifically includes: If the current heating rate R < R_max, increase the actual heating rate R by 1 degree Celsius per minute. Continue to adjust when the heating speed is less than the difference between the maximum heating speed and the target heating speed. Detect whether the difference between the real-time temperature T_real and the heating curve T_ideal under ideal conditions exceeds the allowable deviation △T. When it exceeds △T, fine-tune the heating rate. Dynamically correct the deviation during the heating process based on the information feedback by the temperature control system.
7. A method for producing sintered blue corundum according to claim 6, characterized in that: Dynamically correct the deviation during the heating process based on the information feedback by the temperature control system, specifically including: Calculate the square of the difference between the actual temperature change rate V and the set ideal temperature change rate V_ideal, that is, △V^2 = (V - V_ideal)^2) When △V^2>preset correction condition, the rate correction process is executed, and at the same time, it is monitored whether it exceeds the maximum allowable temperature deviation limit of ±3℃; Recalculate △V^2 after adjustment, and repeat the above steps until the heating is stable or the new correction conditions are reached; The next action of the heating control strategy is determined based on the satisfaction of the correction conditions.
8. A method for producing sintered blue corundum according to claim 7, characterized in that: Repeat the above until the heating is stable or reaches a new correction condition, including: Check whether the reduction of △V decreases three times in a row. If it decreases, it means that it is gradually stabilizing and the correction procedure is stopped; Determine whether the heating duration t reaches the specified total heating duration T. When t ≥ T, it indicates that the heating process has reached the end stage; If the fluctuation range ΔT>±2℃ appears during the constant temperature holding time, the correction cycle needs to be restored until ΔT≤±0.2℃.