Manganese zinc ferrite material as well as preparation method and application thereof
By adjusting the ratio of main and auxiliary components in manganese-zeb ferrite materials and adopting a specific preparation process, the specific temperature coefficient of the material is reduced and the saturation magnetization is improved, and the performance of existing materials in low temperature environments is solved. The problem of instability has expanded its scope of application.
Patent Information
- Application Number
- CN202411002702.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-12-06
AI Technical Summary
The existing manganese-zeb ferrite materials cannot adapt to the extreme conditions of low temperatures, and their specific temperature coefficient is generally higher, limiting their application range.
Using the combination of the main components Fe2O3, ZnO and MnO, and adding CaCO3, SiO2, SnO2, TiO2, Co2O3, Nb2O5 and V2O5 plasma to the auxiliary components, manganese zinc with low specific temperature coefficient was prepared through specific grinding and sintering processes. Ferrite material.
Under negative temperature conditions from -55℃ to 0℃, the specific temperature coefficient of manganese-zeb ferrite material is less than 1.5×10-6/℃, and under positive temperature conditions from 0℃ to 125℃, less than 1×10 -6/℃, the saturation magnetization Bs is higher than 450mT, and the Curie temperature is higher than 200℃, which significantly improves the temperature stability of the material and is suitable for resonant circuits in extremely low temperature environments.
Smart Images

Figure BDA0004962054970000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic materials, and in particular to a manganese-zinc ferrite material and a preparation method and application thereof. Background Art
[0002] Electronic components such as inductors, transformers, filters and chokes with soft ferrite as core components are essential basic elements in industries such as electronic information technology, electric vehicles, photovoltaic industry and smart home. The booming development of the above industries has put forward new requirements for the performance of manganese-zinc soft ferrite. Among them, manganese-zinc ferrite material has the characteristics of high saturation magnetic induction intensity (Bs), high magnetic permeability, low loss, etc., and is a typical and most widely used ferrite material.
[0003] Due to the diversity of working environments of electronic components, the actual working environment temperature has significant differences, and they often need to operate alternately at low and high temperatures. For example, the patent with publication number CN 112194480A discloses a wide temperature, high Bs and low temperature coefficient manganese-zinc ferrite material and its preparation method. The prepared manganese-zinc ferrite material has little change in inductance from -40°C to 125°C, which improves the output stability of the inductor under extreme low temperature / high temperature conditions to a certain extent, but it is still not suitable for extreme environments below -40°C, and the corresponding specific temperature coefficient is generally high. When designing resonant circuits, especially those that need to maintain stability over a wide temperature range, the specific temperature coefficient (Temperature Coefficient of Permeability, TCP) of manganese-zinc ferrite materials is a key parameter. The specific temperature coefficient describes the sensitivity of the material's magnetic permeability to temperature changes. For resonant circuits, the ideal manganese-zinc ferrite material should have a very low specific temperature coefficient, which means that the material's magnetic permeability is affected very little by temperature changes, thereby ensuring that the resonant frequency of the circuit remains relatively constant under different temperature conditions. However, the current low temperature coefficient manganese zinc ferrite products, such as TDK product N48 and Tiantong product TH2, can only adapt to a limited minimum temperature. At the same time, in a low temperature environment, even a small temperature change may cause the inductance of the manganese zinc ferrite material to drop significantly, making it impossible to use normally. In addition, the low Curie temperature and low Bs value of low temperature coefficient manganese zinc ferrite products are also factors that limit their widespread application. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a manganese-zinc ferrite material and a preparation method and use thereof, which solves the technical problems that the current manganese-zinc ferrite material cannot adapt to extreme low temperature conditions and has a generally high temperature coefficient, which limits its application.
[0006] (II) Technical solution
[0007] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0008] In the first aspect, an embodiment of the present invention provides a manganese-zinc ferrite material, comprising a main component and an auxiliary component; the main component is composed of the following components in molar percentage: Fe2O3 52.5-54.5mo1%, ZnO 8-12mo1%, and the rest is MnO; the auxiliary component, based on 100wt% of the main component, includes one or a combination of two or more of 0.02-0.1wt% CaCO3, 0.001-0.01wt% SiO2, 0.1-0.3wt% SnO2, 0.1-0.3wt% TiO2, 0.1-0.3wt% Co2O3, 0.02-0.1wt% Nb2O5 and 0.02-0.1wt% V2O5.
[0009] As a preferred embodiment of the present invention, the main components of the manganese-zinc ferrite material include 53.2-53.8 mol% Fe2O3, 8.5-11 mol% ZnO, and the rest is MnO.
[0010] As a preferred embodiment of the present invention, the manganese-zinc ferrite material, based on 100wt% of the main component, the auxiliary component is one or a combination of two or more of 0.02-0.07wt% CaCO3, 0.002-0.008wt% SiO2, 0.15-0.25wt% SnO2, 0.15-0.25wt% TiO2, 0.12-0.2wt% Co2O3, 0.02-0.05wt% Nb2O5 and 0.02-0.05wt% V2O5.
[0011] As a preferred embodiment of the present invention, the auxiliary component of the manganese-zinc ferrite material is a combination of CaCO3, SnO2, Co2O3 and Nb2O5, or a combination of CaCO3, TiO2, Co2O3 and Nb2O5.
[0012] As a preferred embodiment of the present invention, the manganese-zinc ferrite material, the auxiliary components are 0.05-0.07wt% CaCO3, 0.18-0.25wt% SnO2, 0.12-0.18wt% Co2O3 and 0.02-0.03wt% Nb2O5; or, 0.05-0.07wt% CaCO3, 0.18-0.25wt% TiO2, 0.12-0.18wt% Co2O3 and 0.02-0.03wt% Nb2O5.
[0013] In the second aspect, an embodiment of the present invention provides a method for preparing the manganese-zinc ferrite material described in the first aspect, comprising the following steps: S1. Mixing of main components: weigh the main components, add deionized water, and grind and mix thoroughly to obtain a main component mixture; S2. Pre-burning: After the main component mixture is dried, it is placed at 880-950°C for 1-2 hours, and cooled with the furnace to obtain a pre-burned material; S3. Grinding of the pre-burned material: Add auxiliary components and deionized water to the pre-burned material, grind until the solid D50 particle size is 2.5-3.5μm, and obtain slurry; S4. Granulation: After drying the slurry, granulation is performed; S5. Molding and sintering: The granulated powder is pressed into an annular green body, and then placed in a nitrogen atmosphere for sintering to obtain a manganese-zinc ferrite material.
[0014] As a preferred embodiment of the present invention, in the preparation method of the manganese-zinc ferrite material, in S1 and S3, the grinding method is ball milling; in the ball milling process involved in S1 and S3, the mass ratio of the material to be ground, the ball and the water is 0.8-1.2:2-4:1.0-1.5, and the ball milling time is 40-72min.
[0015] As a preferred embodiment of the present invention, the preparation method of the manganese-zinc ferrite material, in S5, the sintering temperature is 1290-1310°C, and the heat preservation is 3-6h; the density of the annular green body is 2.8-3.0g / cm 3 As a preferred embodiment of the present invention, in the method for preparing the manganese-zinc ferrite material, in S4, after the slurry is dried, polyvinyl alcohol with a mass fraction of 12-15% is added to carry out granulation.
[0016] Among them, polyvinyl alcohol serves as a binder and completely decomposes and volatilizes during the subsequent sintering process.
[0017] In a third aspect, an embodiment of the present invention provides a use of the manganese-zinc ferrite material described in the first aspect, which is used in a resonant circuit.
[0018] (III) Beneficial effects
[0019] The beneficial effects of the present invention are as follows: the magnetocrystalline anisotropy constant (K1) is one of the core parameters affecting the stability of ferrite. Since Zn is a non-magnetic ion, the existing manganese-zinc high-stability ferrite material usually selects a high-content ZnO main component (≥15mol%), which leads to a significant reduction in the Bs value and Curie temperature of the ferrite. The main component of the manganese-zinc ferrite material of the present invention selects an iron formula, reduces the amount of ZnO, and further dopes Co in the auxiliary component. 2+ 、Ti 4+ Sn 4+Plasma effectively compensates for the negative K1 of the main component, greatly reducing the dependence of the material's magnetocrystalline anisotropy on temperature, and achieving the temperature stability of the ferrite material's magnetic permeability. The specific temperature coefficient of the prepared manganese-zinc ferrite material under negative temperature conditions of -55°C to 0°C is less than 1.5×10 -6 / ℃, the specific temperature coefficient (temperature coefficient of magnetic permeability) is less than 1×10 -6 / ℃, the room temperature saturation magnetization (Bs) measured at 1194A / m and 50Hz is higher than 450mT, and the Curie temperature is higher than 200℃. Compared with the prior art, the manganese-zinc ferrite material has good temperature stability of magnetic permeability in a wide temperature range, is adaptable to extreme low temperature environments, and has a further expanded scope of application, and is particularly suitable for use in resonant circuits working in extreme low temperature environments.
[0020] The manganese-zinc ferrite material provided by the present invention comprises 52.5-54.5 mol% of Fe2O3, 8-12 mol% of ZnO, and the rest is MnO. The auxiliary components, based on 100 wt% of the main components, include one or a combination of two or more of 0.02-0.07 wt% of CaCO3, 0.001-0.01 wt% of SiO2, 0.1-0.3 wt% of SnO2, 0.1-0.3 wt% of TiO2, 0.1-0.3 wt% of Co2O3, 0.02-0.1 wt% of Nb2O5, and 0.02-0.1 wt% of V2O5. The manganese-zinc ferrite material prepared by using the above components and corresponding dosage ratios has a low specific temperature coefficient, wherein, under a relatively extreme low temperature environment of -55°C, the specific temperature coefficient is concentrated in the range of (0.65-0.9)×10 -6 / ℃; under the conditions of 1194A / m and 50Hz, the saturation magnetic flux density Bs is high, mainly concentrated in 452-465mT. It can be seen that the manganese-zinc ferrite material of the present invention has excellent overall performance and is a manganese-zinc ferrite material with good temperature stability in a wide temperature range.
[0021] In the manganese-zinc ferrite material and its preparation method, the main component mixture is pre-burned at 880-950°C for 1-2 hours, which can promote the initial reaction between the raw materials and make the oxides of iron, manganese and zinc begin to form a ferrite structure. In this temperature range, the solid phase reaction begins to occur, which helps to form a more uniform microstructure. The higher the temperature in this temperature range, the lower the specific temperature coefficient of the corresponding manganese-zinc ferrite material at -55°C.
[0022] Add auxiliary ingredients and deionized water to the pre-sintered material, and grind until solid D 50The particle size is 2.5-3.5μm, which is conducive to accelerating the diffusion rate in the subsequent sintering process, reducing the porosity in the sintering process, improving the density and magnetic properties of the material, and also helps to form a more continuous magnetic domain boundary, which has a positive effect on improving the magnetic permeability of the material and reducing the hysteresis loss. In the molding stage, the fluidity and compressibility of the material can be improved, making the material easier to be pressed and molded, while reducing cracks and delamination in the molding process. DETAILED DESCRIPTION
[0023] In order to better explain the present invention and facilitate understanding, the present invention is described in detail through specific implementation methods.
[0024] The present invention provides a manganese-zinc ferrite material and a preparation method and use thereof, which aims to solve the technical problems that the current manganese-zinc ferrite material cannot adapt to extreme low temperature conditions and has a generally high temperature coefficient, which limits its application. The main component of the manganese-zinc ferrite material of the present invention is an iron formula, and the amount of ZnO is reduced, and Co is further doped in the auxiliary component. 2+ 、Ti 4+ Sn 4+ Plasma effectively compensates for the negative K1 of the main component, greatly reducing the dependence of the material's magnetocrystalline anisotropy on temperature, and achieving the temperature stability of the ferrite material's magnetic permeability. The specific temperature coefficient of the prepared manganese-zinc ferrite material under negative temperature conditions of -55°C to 0°C is less than 1.5×10 -6 / ℃, the specific temperature coefficient (temperature coefficient of magnetic permeability) is less than 1×10 -6 / ℃, the room temperature saturation magnetization (Bs) measured at 1194A / m and 50Hz is higher than 450mT, and the Curie temperature is higher than 200℃. Compared with the prior art, the manganese-zinc ferrite material has good temperature stability of magnetic permeability in a wide temperature range, is adaptable to extreme low temperature environments, and has a further expanded scope of application, and is particularly suitable for use in resonant circuits working in extreme low temperature environments.
[0025] In order to better understand the above technical scheme, exemplary embodiments of the present invention will be described in more detail below. Although the present invention provides exemplary embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a clearer and more thorough understanding of the present invention, and to be able to fully convey the scope of the present invention to those skilled in the art.
[0026] Example 1
[0027] This embodiment provides a method for preparing a manganese-zinc ferrite material, and the specific steps are as follows:
[0028] (1) Mixing the main components: weigh the main components (wherein Fe2O3, ZnO and MnO (actually Mn3O4, expressed as MnO) are 53.5 mol%, 11 mol% and 35.5 mol% respectively), add deionized water, and mill in a planetary ball mill for 40 min, wherein the mass ratio of material, ball and water is 1:3.5:1.2, and mix thoroughly by ball milling to obtain a main component mixture;
[0029] (2) Pre-burning: The powder of the main component mixture is dried and kept at 920°C for 2 hours, and then cooled in the furnace to obtain the pre-burned material;
[0030] (3) Secondary ball milling: Based on 100 wt% of the main component in (1), the auxiliary components are CaCO3, TiO2, Co2O3 and Nb2O5, with amounts of 0.05%, 0.2%, 0.15% and 0.02% respectively; the pre-sintered material and the above auxiliary components and deionized water are added to the ball mill, and the ball milling is performed in a planetary ball mill. The mass ratio of material, ball and water is 1:3.5:1.2, and the ball milling time is 1 h, until the powder D50 particle size is less than 3.5 μm, to obtain a slurry;
[0031] (4) Granulation: After drying the slurry, add 12% by mass of polyvinyl alcohol (PVA) for granulation, wherein 24 g of 12% polyvinyl alcohol (PVA) is added for every 200 g of the dried slurry;
[0032] (5) Molding and sintering: The granulated powder is pressed into a T20*10*5 annular green body with a green body density of 3.0 g / cm 3 ;
[0033] (6) Sintering: The green body was sintered under nitrogen protection at a sintering temperature of 1300°C for 5 hours. The temperature was kept at 5% oxygen partial pressure during the holding stage. The temperature was cooled to below 200°C by the equilibrium atmosphere method and the sample ring was taken out to obtain the manganese-zinc ferrite material.
[0034] Example 2
[0035] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the auxiliary components in step (3) are CaCO3, TiO2, Co2O3 and Nb2O5, which are 0.02%, 0.25%, 0.12% and 0.02% respectively.
[0036] Example 3
[0037] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the auxiliary components in step (3) are CaCO3, TiO2, Co2O3 and Nb2O5, which are 0.07%, 0.15%, 0.2% and 0.02% respectively.
[0038] Example 4
[0039] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the auxiliary components in step (3) are CaCO3, TiO2, Co2O3 and V2O5, which are 0.05%, 0.2%, 0.15% and 0.02% respectively.
[0040] Example 5
[0041] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the main components in step (1) are Fe2O3, ZnO and MnO, and the amounts used are 54.5 mol%, 10 mol% and 35.5 mol% respectively;
[0042] In step (3), based on 100wt% of the main component in (1), the auxiliary components CaCO3, TiO2, Co2O3 and Nb2O5 are 0.05%, 0.1%, 0.18% and 0.02% respectively.
[0043] Example 6
[0044] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the amounts of the main components Fe2O3, ZnO and MnO in step (1) are 54 mol%, 8 mol% and 38 mol% respectively;
[0045] In step (3), based on 100wt% of the main component in (1), the auxiliary components CaCO3, TiO2, Co2O3 and Nb2O5 are 0.05%, 0.2%, 0.25% and 0.02% respectively.
[0046] Example 7
[0047] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the amounts of the main components Fe2O3, ZnO and MnO in step (1) are 53.5 mol%, 12 mol% and 34.5 mol% respectively;
[0048] In step (3), based on 100wt% of the main component in (1), the auxiliary components CaCO3, TiO2, Co2O3 and Nb2O5 are 0.06%, 0.23%, 0.1% and 0.02% respectively.
[0049] Example 8
[0050] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the amounts of the main components Fe2O3, ZnO and MnO in step (1) are 52.5 mol%, 9 mol% and 38.5 mol% respectively;
[0051] In step (3), based on 100wt% of the main component in (1), the auxiliary components CaCO3, TiO2, Co2O3 and Nb2O5 are 0.04%, 0.3%, 0.15% and 0.02% respectively.
[0052] Example 9
[0053] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the pre-firing temperature in step (2) is 900° C.
[0054] Example 10
[0055] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the pre-firing temperature in step (2) is 950°C.
[0056] Embodiment 11
[0057] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the mass ratio of material, balls, and water in the ball milling in step (3) is 1:3:1.2, and the ball milling time is 1 hour.
[0058] Example 12 provides a method for preparing a manganese-zinc ferrite material. Compared with Example 11, the difference is that the ball milling time in step (3) is 40 minutes.
[0059] Embodiment 13
[0060] This embodiment provides a method for preparing a manganese-zinc ferrite material. Compared with Embodiment 1, the difference is that the green density in step (5) is 2.8 g / cm 3 .
[0061] Comparative Example 1
[0062] Compared with Example 1, the difference between this comparative example and Example 1 is that in step (3), based on 100wt% of the main component in (1), the auxiliary components CaCO3, TiO2, Co2O3 and Nb2O5 are 0.1%, 0.4%, 0.05% and 0.02% respectively.
[0063] Comparative Example 2
[0064] The difference between this comparative example and Example 1 is that in step (3), based on 100wt% of the main component in (1), Co2O3 is removed from the auxiliary components, and the other auxiliary components remain unchanged.
[0065] Comparative Example 3
[0066] The difference between this comparative example and Example 1 is that in step (3), based on 100 wt% of the main component in (1), TiO2 is removed from the auxiliary components, and the other auxiliary components remain unchanged.
[0067] Comparative Example 4
[0068] The difference between this comparative example and Example 1 is that in step (3), based on 100wt% of the main component in (1), Nb2O5 is removed from the auxiliary components, and the other auxiliary components remain unchanged.
[0069] Comparative Example 5
[0070] The difference between this comparative example and Example 1 is that the amounts of the main components Fe2O3, ZnO and MnO in step (1) are 52 mol%, 13 mol% and 35 mol%, respectively.
[0071] Comparative Example 6
[0072] The difference between this comparative example and Example 1 is that the amounts of the main components Fe2O3, ZnO and MnO in step (1) are 55 mol%, 7 mol% and 38 mol%, respectively.
[0073] Comparative Example 7
[0074] The difference between this comparative example and Example 1 is that the pre-firing temperature in step (2) is 980°C.
[0075] Comparative Example 8
[0076] The difference between this comparative example and Example 1 is that the pre-firing temperature in step (2) is 850°C.
[0077] For the manganese-zinc ferrite materials prepared in the above embodiments and comparative examples, the inductance values of the sample rings were tested in turn; then the magnetic permeability of the manganese-zinc ferrite materials, as well as the temperature coefficient and Curie temperature at different temperatures were tested under the conditions of 25°C, 10kHz, and 100mV; further, the saturation magnetic flux density of the sample ring was tested under the conditions of 1194A / m and 50Hz. The test results of relevant performance indicators are shown in Table 1.
[0078] Table 1
[0079]
[0080] It can be seen from Table 1 that Example 1 is the best example. The specific temperature coefficient of the prepared manganese-zinc ferrite material is lower as a whole, the magnetic permeability and saturation magnetic flux density Bs are the highest, the Curie temperature is the highest, and the overall comprehensive performance of the manganese-zinc ferrite material is the best.
[0081] Comparing Example 2, Example 3, and Example 4 with Example 1, it can be seen that, among the auxiliary components, fine-tuning the ratio between the various components will have a significant impact on the temperature coefficient. This is mainly because different doping ratios compensate the main component K1 value differently, resulting in changes in the difficulty of domain wall movement and magnetic domain rotation, which further affects the change of magnetic permeability at different temperatures.
[0082] Comparison of Comparative Examples 2, 3 and 4 with Example 1 shows that, when one of the auxiliary components is missing, the specific temperature coefficient of the prepared manganese-zinc ferrite material is significantly increased and the magnetic permeability is significantly decreased.
[0083] Comparison of Example 5, Example 6, Example 7 and Example 8 with Example 1 shows that different proportions of main components have an impact on Bs, Curie temperature and specific temperature coefficient of the manganese-zinc ferrite material.
[0084] Comparing Example 10 and Example 11 with Example 1, it can be seen that the best effect is achieved when the pre-firing temperature is 920°C; at the same time, when the pre-firing temperature range of Example 10, Example 11 and Example 1 is compared with Comparative Examples 7 and 8, it can be seen that when the pre-firing temperature range exceeds the range of 880-950°C, the temperature coefficient of the manganese-zinc ferrite material will increase significantly, and the magnetic permeability will also decrease significantly. This is because too low a pre-firing temperature will lead to too low a degree of solid-phase reaction of the pre-firing powder, too high an activity, and secondary crystallization and abnormal grain growth will occur in the subsequent sintering process, making the ferrite microstructure seriously uneven and the magnetic properties significantly damaged. However, too high a pre-firing temperature will cause an excessive degree of solid-phase reaction of the powder, too high a hardness of the pre-firing material, increase the difficulty of crushing the secondary ductile iron, and make the grain size after sintering too large and uneven, the microstructure poor, and the magnetic properties poor.
[0085] Comparing Example 12 and Example 13 with Example 1, it can be seen that reducing the number of grinding balls or reducing the ball milling time will affect the final ball milling effect, that is, insufficient ball milling will lead to an increase in the temperature coefficient of the manganese-zinc ferrite material and a decrease in the magnetic permeability.
[0086] By comparing Example 14 with Example 1, it can be seen that, within a certain range, a lower green density after molding will optimize the specific temperature coefficient, but Bs will be significantly reduced. This is because a low green density will reduce the contact area of the particles, and the size of the grains during sintering will be smaller and the grain boundaries will be thicker, which will increase the difficulty of domain wall movement, making it difficult for the magnetic permeability to change significantly with temperature.
[0087] Comparison between Comparative Examples 5 and 6 and Example 1 shows that the specific temperature coefficient of the manganese-zinc ferrite material obtained when the proportion of the main component exceeds the scope of the technical solution of the present invention is very high.
[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A manganese-zinc ferrite material, It is characterized in that Includes main components and auxiliary components; The main component is composed of the following components in molar percentage: Fe 2 O 3 52.5-54.5 mol%, ZnO 8-12 mol%, the rest is MnO; The auxiliary component, based on 100wt% of the main component, includes 0.02-0.1wt% CaCO 3 0.001-0.01wt%SiO 2 , 0.1-0.3wt% SnO 2 , 0.1-0.3wt%TiO 2 , 0.1-0.3wt% Co 2 O 3 0.02-0.1wt% Nb 2 O 5 and 0.02-0.1wt%V 2 O 5 One or a combination of two or more.
2. The manganese-zinc ferrite material according to claim 1, It is characterized in that The main component includes Fe 2 O 3 53.2-53.8mo1%, ZnO 8.5-11mo1%, and the rest is MnO.
3. The manganese-zinc ferrite material according to claim 2, It is characterized in that Based on 100wt% of the main component, the auxiliary component is 0.02-0.07wt% CaCO 3 0.002-0.008wt%SiO 2 , 0.15-0.25wt% SnO 2 , 0.15-0.25wt%TiO 2 0.12-0.2wt% Co 2 O 3 0.02-0.05wt% Nb 2 O 5 and 0.02-0.05wt%V 2 O 5 One or a combination of two or more.
4. The manganese-zinc ferrite material according to any one of claims 1 to 3, It is characterized in that The auxiliary component is CaCO 3 SnO 2 、Co 2 O 3 and Nb 2 O 5 A combination of, or, CaCO 3 、TiO 2 、Co 2 O 3 and Nb 2 O 5 combination.
5. The manganese-zinc ferrite material according to any one of claims 4, It is characterized in that The auxiliary component is 0.05-0.07wt% CaCO 3 , 0.18-0.25wt% SnO 2 , 0.12-0.18wt%Co 2 O 3 and 0.02-0.03wt% Nb 2 O 5 ; Alternatively, 0.05-0.07 wt% CaCO 3 , 0.18-0.25wt%TiO 2 , 0.12-0.18wt%Co 2 O 3 and 0.02-0.03wt% Nb 2 O 5 .
6. A method for preparing the manganese-zinc ferrite material according to any one of claims 1 to 5, It is characterized in that The following steps are involved: S1. Mixing the main components: weigh the main components, add deionized water, and grind and mix thoroughly to obtain a main component mixture; S2, pre-burning: After the main component mixture is dried, it is placed at 880-950℃ for 1-2 hours and cooled with the furnace to obtain the pre-burned material; S3, pre-burned material grinding: adding auxiliary components and deionized water to the pre-burned material, grinding until the solid D50 particle size is 2.5-3.5 μm, to obtain a slurry; S4, granulation: drying the slurry and then granulating it; S5. Molding and sintering: The granulated powder is pressed into a ring-shaped green body, and then sintered in a nitrogen atmosphere to obtain a manganese-zinc ferrite material.
7. The method for preparing the manganese-zinc ferrite material according to claim 6, It is characterized in that In S1 and S3, the grinding method was ball milling; In the ball milling processes involved in S1 and S3, the mass ratios of the material to be ground, the balls and the water are all 0.8-1.2:2-4:1.0-1.5, and the ball milling time is all 40-72 min.
8. The method for preparing the manganese-zinc ferrite material according to claim 6, It is characterized in that In S5, the sintering temperature is 1290-1310°C and kept at this temperature for 3-6h; The density of the ring-shaped green body is 2.8-3.0g / cm 3 .
9. The method for preparing the manganese-zinc ferrite material according to claim 6, It is characterized in that In S4, after the slurry is dried, polyvinyl alcohol with a mass fraction of 12-15% is added to perform granulation.
10. The manganese-zinc ferrite material according to any one of claims 1 to 5, used in a resonant circuit.
Citation Information
Patent Citations
Manganese-zinc ferrite material with wide temperature range, high Bs and low temperature coefficient and preparation method thereof
CN112194480A
Wide-temperature wide-band magnetic manganese-zinc ferrite and preparation method thereof
CN106278228A
MnZn high permeability material with wide temperature, broadband and low temperature coefficient and preparation method thereof
CN107500746A
Manganese-zinc ferrite material with wide temperature range and low power consumption and preparation method thereof
CN112408969A
Manganese-zinc ferrite material with ultra-wide temperature, low power consumption, magnetic conductivity and temperature stability and preparation method of manganese-zinc ferrite material
CN115650718A