Hfnium-zirconium-carbon ternary complex-phase ceramic precursor and preparation method thereof
By reacting hafnium tetrachloride and zirconium tetrachloride with sodium alkyl in anhydrous and oxygen-free environment, copolymerizing with polyolefins, hafnium zirconium carbon ternary composite ceramic precursor was prepared, and hafnium in the prior art was solved The complex and costly preparation of zirconium carbon ceramics has achieved improved high temperature mechanical properties and increased ceramic yields, and is suitable for aerospace materials.
Patent Information
- Application Number
- CN202411167434.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
AI Technical Summary
The existing hafnium zirconium carbon ceramic preparation methods are complex, the product quality is easily affected by raw materials and temperature, and the cost is high, making it difficult to meet the performance needs of aerospace materials.
Hafnium tetrachloride and zirconium tetrachloride react with sodium alkyl containing electron-rich groups in anhydrous and oxygen-free environment to produce hafnium tetrachloride and zirconium dichloride, and then copolymerize with polyolefin. The hafnium zirconium carbon ternary composite ceramic precursor was prepared, which improved the stability and high-temperature mechanical properties of the ceramic.
The high-temperature mechanical properties of hafnium zirconium carbon ternary composite ceramic precursor have been improved, the ceramic yield has been increased, the preparation process has been simplified, and the cost has been reduced. It is suitable for the application of aerospace materials.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic materials, and in particular to a hafnium-zirconium-carbon ternary composite ceramic precursor and a preparation method thereof. Background Art
[0002] Hafnium zirconium carbon ceramics are an important high-temperature structural material. Due to its excellent heat resistance and chemical stability, hafnium zirconium carbon ceramics are widely used in high-temperature components and refractory materials. It overcomes the fatal weakness of single-phase ceramic materials, which are brittle, and has excellent properties such as low density, ternary complex phase, high strength, oxidation resistance and ablation resistance. As an aerospace material, it has been used in the rudders of supersonic aircraft.
[0003] At present, common methods for preparing hafnium zirconium carbon ceramics include solid phase reaction method, sol-gel method and plasma spraying method. The solid phase reaction method prepares hafnium zirconium carbon ceramics by mixing hafnium and zirconium powders with a carbon source at high temperature for reaction. However, the preparation process of this method is complicated, and the product quality is greatly affected by the quality of the raw materials and the reaction temperature (when the reaction temperature is different, the crystal form of the product changes significantly). The sol-gel method is to dissolve metal salts and organic matter in a solvent to form a gel and then dry and heat treat to obtain ceramics. Although this method can obtain higher ceramic purity and uniformity, the equipment and preparation process used are relatively complex and the cost is high. The plasma spraying method is to spray metal powder and carbon source directly on the substrate through a high-temperature airflow generated by plasma to form a ceramic coating. This method is suitable for preparing ceramic coatings of complex shapes, but the preparation process is complicated. Summary of the invention
[0004] In view of this, one of the purposes of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing a hafnium-zirconium-carbon ternary composite ceramic precursor. The hafnium-zirconium-carbon ternary composite ceramic precursor prepared by this preparation method has stable quality, high melting point, high oxidation resistance, stable high-temperature mechanical properties, simple preparation process, low cost, and high ceramic yield, which meets the performance requirements of aerospace materials.
[0005] In order to achieve one of the above purposes, the present invention adopts the following technical solutions:
[0006] A method for preparing a hafnium-zirconium-carbon ternary composite ceramic precursor, the preparation method comprising the following steps:
[0007] Step S1, in an anhydrous and oxygen-free environment, in a mass ratio of 1 to 10:10 to 1, reacting hafnium tetrachloride and an alkyl sodium containing an electron-rich group at a temperature of -10 to -5°C for 2 to 4 hours to obtain hafnium dichloride;
[0008] Step S2, reacting hafnium dichloride and an alkyl sodium containing an electron-rich group at a temperature of -25 to -5°C for 1 to 6 hours in a mass ratio of 1 to 3:1 to generate a hafnium intermediate;
[0009] Step S3, reacting the hafnium intermediate and the organic solvent at a temperature of 50 to 70° C. for 3 to 7 hours in a mass ratio of 1:3 to 6 to generate a hafnium precursor;
[0010] Step S4, in an anhydrous and oxygen-free environment, react zirconium tetrachloride, a reducing agent and an alkyl sodium containing an electron-rich group at a temperature of -10 to -5°C for 2 to 4 hours in a mass ratio of 1 to 3:1:3 to 6 to obtain zirconocene dichloride;
[0011] Step S5, reacting zirconocene dichloride, alkyl sodium containing electron-rich groups and an organic solvent at a temperature of -25 to 70° C. for 1 to 6 hours in a mass ratio of 1 to 3:1 to 3 to 18 to generate a zirconium precursor;
[0012] Step S6, copolymerize the hafnium precursor, the zirconium precursor and the polyolefin with a molecular weight of 7000-300000 at a temperature of 50-70°C for 3-5 hours in a mass ratio of 1:1-4:1-5, let stand for 8-12 hours, and filter to obtain a hafnium-zirconium-carbon ternary composite ceramic precursor.
[0013] Furthermore, in the step S1, the mass ratio of the hafnium chloride to the alkyl sodium is 3-7:7-3.
[0014] Further, in step S1, step S2, step S4 and step S5, the electron-rich group is one or more of methyl, ethyl, vinyl, phenyl, cyclopentyl, propenyl and propynyl;
[0015] The alkyl sodium is one or more of methylcyclopentyl sodium, ethylcyclohexyl sodium, allyl sodium, propynyl sodium, propynyl sodium bromide, methylvinyl sodium chloride, allyl sodium bromide, propynyl sodium iodide, propynyl sodium chloride, and cyclopentylmethyl sodium.
[0016] Furthermore, in step S3 and step S5, the organic solvent is one or more of benzene, toluene, dichloromethane, tetrahydrofuran, DMF, and N-methylpyrrolidone.
[0017] Furthermore, in step S4, the reducing agent is one or more of hydrogen, carbon monoxide, hydrogen sulfide, ethanol, formic acid, oxalic acid, and sodium borohydride.
[0018] Furthermore, in the step S5, the mass ratio of the zirconocene dichloride, the alkyl sodium containing electron-rich groups and the organic solvent is 1-3:1:8-14.
[0019] Furthermore, in the step S6, the mass ratio of hafnium to zirconium in the hafnium-zirconium-carbon ternary composite ceramic precursor is 1:1-4.
[0020] Furthermore, in the step S6, the molecular weight of the polyolefin is 10,000 to 15,000, preferably 30,000 to 200,000, and preferably 80,000 to 100,000.
[0021] Furthermore, in step S6, the polyolefin is one or more of polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, polyhexene, polyoctene, and polynonene.
[0022] In order to achieve the second objective above, the present invention adopts the following technical solution:
[0023] A hafnium-zirconium-carbon ternary composite ceramic precursor is prepared by the above-mentioned preparation method.
[0024] The beneficial effects of the present invention are:
[0025] The invention realizes the transition from intergranular fracture to crystal-linked fracture of a hafnium-zirconium-carbon ternary composite ceramic precursor through copolymerization of a hafnium precursor, a zirconium precursor and a polyolefin, and improves the performance at high temperature instead of decreasing, thereby effectively improving the mechanical properties (high-temperature mechanical properties) of the hafnium-zirconium-carbon ternary composite ceramic precursor at high temperature, and has important application prospects in the field of aerospace. The invention allows the three phases to be evenly mixed by standing, thereby improving the ceramic yield. The invention utilizes hafnium and zirconium of the same family, and adopts zirconium elements to replace hafnium elements to prepare a solid solution, which can remain stable at high temperatures. With the increase of the proportion of zirconium elements, the initial melting temperature of the solid solution decreases non-linearly, thereby realizing the regulation of the rheological properties of the precursor by changing the proportion of refractory metal hafnium and zirconium, thereby improving the processing performance of the hafnium-zirconium-carbon ternary composite ceramic precursor, and can be used to prepare ternary composite coatings, fiber reinforcements and ceramic-based composite matrixes. The viscosity of the hafnium-zirconium-carbon ternary composite ceramic precursor is 100-500 mPa·s. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with specific implementation modes.
[0027] Embodiment 1:
[0028] 1. In an anhydrous and oxygen-free environment, add hafnium tetrachloride and methylcyclopentyl sodium in a 1:1 mass ratio into a reaction vessel and react at -10°C for 2 hours to obtain hafnium dichloride.
[0029] 2. Then, according to a mass ratio of 1:1, methylcyclopentyl sodium was added to dichlorodichlorobenzene and reacted at -25°C for 1 hour to generate a hafnium intermediate. Then, according to a mass ratio of 1:3, the hafnium intermediate and benzene were reacted at 50°C for 3 hours to generate a hafnium precursor.
[0030] 3. In an anhydrous and oxygen-free environment, zirconium tetrachloride and carbon monoxide are added to a reaction vessel in a mass ratio of 1:1:3, and then methylcyclopentyl sodium is added to react at -10°C for 2h to obtain zirconocene dichloride.
[0031] 4. According to the mass ratio of 1:1:3, dichloromonocyclopentyl zirconium, methylcyclopentyl sodium and benzene were reacted at -25°C for 1 hour to generate an (alkyl) zirconium precursor.
[0032] 5. According to the mass ratio of 1:1:1, the hafnium precursor and the alkyl zirconium precursor were mixed and stirred, and polyethylene with a molecular weight of 7000 was added to copolymerize at a temperature of 50°C for 3 hours, and then allowed to stand for 8 hours and filtered to obtain a hafnium-zirconium-carbon ternary composite ceramic precursor. The mass ratio of hafnium to zirconium in the hafnium-zirconium-carbon ternary composite ceramic precursor is 1:1.
[0033] Under argon atmosphere, the hafnium zirconium carbon ternary composite ceramic precursor of this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yields at 1400°C and 1600°C were 45.46% and 40.55%, respectively. The bending strengths of the hafnium zirconium carbon ternary composite ceramic precursor at 900°C and 1600°C were 510MPa and 682MPa, respectively, and the viscosity was 200mPa·s.
[0034] Embodiment 2:
[0035] 1. In an anhydrous and oxygen-free environment, add hafnium tetrachloride and ethylcyclohexyl sodium in a reaction vessel in a mass ratio of 10:1 and react at -5°C for 4 hours to obtain hafnium dichloride.
[0036] 2. Then, add ethylcyclohexyl sodium to dichloro hafnium in a mass ratio of 3:1 and react at -5°C for 6 hours to generate a hafnium intermediate. Then, react the hafnium intermediate with toluene at a mass ratio of 1:6 at 70°C for 7 hours to generate a hafnium precursor.
[0037] 3. In an anhydrous and oxygen-free environment, zirconium tetrachloride and hydrogen sulfide are added to a reaction vessel in a mass ratio of 3:1:6, and then ethylcyclohexyl sodium is added to react at -5°C for 4 hours to obtain zirconocene dichloride.
[0038] 4. According to the mass ratio of 3:1:18, dichloromonocyclopentadienyl zirconium, ethylcyclohexyl sodium and toluene were reacted at -70°C for 6 hours to generate an (alkyl) zirconium precursor.
[0039] 5. According to the mass ratio of 1:4:5, the hafnium precursor and the alkyl zirconium precursor were mixed and stirred, and polypropylene with a molecular weight of 300,000 was added to copolymerize at a temperature of 70°C for 5 hours, and then allowed to stand for 12 hours, and filtered to obtain a hafnium-zirconium-carbon ternary composite ceramic precursor. The mass ratio of hafnium to zirconium in the hafnium-zirconium-carbon ternary composite ceramic precursor is 1:4.
[0040] Under argon atmosphere, the hafnium zirconium carbon ternary composite ceramic precursor of this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yields at 1400°C and 1600°C were 45.74% and 38.54%, respectively. The bending strengths of the hafnium zirconium carbon ternary composite ceramic precursor at 900°C and 1600°C were 512MPa and 684MPa, respectively, and the viscosity was 100mPa·s.
[0041] Embodiment 3:
[0042] 1. In an anhydrous and oxygen-free environment, add hafnium tetrachloride and allyl sodium in a mass ratio of 7:3 into a reaction vessel and react at -7°C for 3 hours to obtain hafnium dichloride.
[0043] 2. Then, according to the mass ratio of 2:1, add allyl sodium to dichlorodichlorohexene and react at -10°C for 2 hours to generate a hafnium intermediate. Then, according to the mass ratio of 1:4, react the hafnium intermediate with dichloromethane at 60°C for 5 hours to generate a hafnium precursor.
[0044] 3. In an anhydrous and oxygen-free environment, zirconium tetrachloride and ethanol are added to a reaction vessel in a mass ratio of 2:1:4, and then allyl sodium is added to react at -7°C for 3 hours to obtain dichlorobis(cyclopentadienyl)zirconium.
[0045] 4. According to the mass ratio of 2:1:10, dichloromonocyclopentadienyl zirconate, allyl sodium and dichloromethane were reacted at 20°C for 4 hours to generate an alkyl zirconium precursor.
[0046] 5. According to the mass ratio of 1:3:2, the hafnium precursor and the alkyl zirconium precursor were mixed and stirred, and polybutene with a molecular weight of 10,000 was added to copolymerize at a temperature of 60°C for 4 hours, and then allowed to stand for 10 hours and filtered to obtain a hafnium-zirconium-carbon ternary composite ceramic precursor. The mass ratio of hafnium to zirconium in the hafnium-zirconium-carbon ternary composite ceramic precursor is 1:3.
[0047] Under argon atmosphere, the hafnium zirconium carbon ternary composite ceramic precursor of this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yields at 1400°C and 1600°C were 45.15% and 39.89%, respectively. The bending strengths of the hafnium zirconium carbon ternary composite ceramic precursor at 900°C and 1600°C were 516MPa and 687MPa, respectively, and the viscosity was 300mPa·s.
[0048] Embodiment 4:
[0049] 1. In an anhydrous and oxygen-free environment, add hafnium tetrachloride and sodium propynyl in a mass ratio of 3:7 into a reaction vessel and react at -8°C for 3 hours to obtain hafnium dichloride.
[0050] 2. Sodium propargyl is added to hafnium dichloride at a mass ratio of 2:1 and reacted at -20°C for 4 hours to generate a hafnium intermediate. The hafnium intermediate and tetrahydrofuran are reacted at a mass ratio of 1:5 at 65°C for 4 hours to generate a hafnium precursor.
[0051] 3. In an anhydrous and oxygen-free environment, zirconium tetrachloride and formic acid are added to a reaction vessel in a mass ratio of 2:1:5, and then sodium propynyl is added to react at -8°C for 3 hours to obtain zirconocene dichloride.
[0052] 4. According to the mass ratio of 2:1:16, dichloromonocyclopentadienyl zirconium, sodium propynyl and tetrahydrofuran were reacted at 60°C for 5 hours to generate an alkyl zirconium precursor.
[0053] 5. According to the mass ratio of 1:2:4, the hafnium precursor and the alkyl zirconium precursor were mixed and stirred, and polyisobutylene with a molecular weight of 200,000 was added to copolymerize at a temperature of 65°C for 4 hours, and then allowed to stand for 9 hours and filtered to obtain a hafnium-zirconium-carbon ternary composite ceramic precursor. The mass ratio of hafnium to zirconium in the hafnium-zirconium-carbon ternary composite ceramic precursor is 1:2.
[0054] Under argon atmosphere, the hafnium zirconium carbon ternary composite ceramic precursor of this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yields at 1400°C and 1600°C were 45.65% and 39.53%, respectively. The bending strengths of the hafnium zirconium carbon ternary composite ceramic precursor at 900°C and 1600°C were 520MPa and 683MPa, respectively, and the viscosity was 500mPa·s.
[0055] The above examples are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the best embodiment, a person skilled in the art should understand that the technical solution of the present invention can still be modified or replaced by equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a hafnium-zirconium-carbon ternary composite ceramic precursor, characterized in that: The preparation method comprises the following steps: Step S1, in an anhydrous and oxygen-free environment, in a mass ratio of 1 to 10:10 to 1, reacting hafnium tetrachloride and an alkyl sodium containing an electron-rich group at a temperature of -10 to -5°C for 2 to 4 hours to obtain hafnium dichloride; Step S2, reacting hafnium dichloride and an alkyl sodium containing an electron-rich group at a temperature of -25 to -5°C for 1 to 6 hours in a mass ratio of 1 to 3:1 to generate a hafnium intermediate; Step S3, reacting the hafnium intermediate and the organic solvent at a temperature of 50 to 70° C. for 3 to 7 hours in a mass ratio of 1:3 to 6 to generate a hafnium precursor; Step S4, in an anhydrous and oxygen-free environment, react zirconium tetrachloride, a reducing agent and an alkyl sodium containing an electron-rich group at a temperature of -10 to -5°C for 2 to 4 hours in a mass ratio of 1 to 3:1:3 to 6 to obtain zirconocene dichloride; Step S5, reacting zirconocene dichloride, alkyl sodium containing electron-rich groups and an organic solvent at a temperature of -25 to 70° C. for 1 to 6 hours in a mass ratio of 1 to 3:1 to 3 to 18 to generate a zirconium precursor; Step S6, copolymerize the hafnium precursor, the zirconium precursor and the polyolefin with a molecular weight of 7000-300000 at a temperature of 50-70°C for 3-5 hours in a mass ratio of 1:1-4:1-5, let stand for 8-12 hours, and filter to obtain a hafnium-zirconium-carbon ternary composite ceramic precursor.
2. The preparation method according to claim 1, characterized in that: In the step S1, the mass ratio of the hafnium chloride to the alkyl sodium is 3-7:7-3.
3. The preparation method according to claim 2, characterized in that: In the step S1, step S2, step S4 and step S5, the electron-rich group is one or more of methyl, ethyl, vinyl, phenyl, cyclopentyl, propenyl and propynyl; The alkyl sodium is one or more of methylcyclopentyl sodium, ethylcyclohexyl sodium, allyl sodium, propynyl sodium, propynyl sodium bromide, methylvinyl sodium chloride, allyl sodium bromide, propynyl sodium iodide, propynyl sodium chloride, and cyclopentylmethyl sodium.
4. The preparation method according to claim 3, characterized in that: In step S3 and step S5, the organic solvent is one or more of benzene, toluene, dichloromethane, tetrahydrofuran, DMF, and N-methylpyrrolidone.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S4, the reducing agent is one or more of carbon monoxide, hydrogen sulfide, ethanol, formic acid, oxalic acid, and sodium borohydride.
6. The preparation method according to claim 5, characterized in that: In the step S5, the mass ratio of the zirconocene dichloride, the alkyl sodium containing electron-rich groups and the organic solvent is 1-3:1:8-14.
7. The preparation method according to claim 6, characterized in that: In the step S6, the mass ratio of hafnium to zirconium in the hafnium-zirconium-carbon ternary composite ceramic precursor is 1:1-4.
8. The preparation method according to claim 7, characterized in that: In the step S6, the molecular weight of the polyolefin is 30,000 to 200,000.
9. The preparation method according to claim 8, characterized in that: In the step S6, the polyolefin is one or more of polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, polyhexene, polyoctene, and polynonene.
10. A hafnium-zirconium-carbon ternary composite ceramic precursor, characterized in that: The hafnium-zirconium-carbon ternary composite ceramic precursor is prepared by the preparation method described in claims 1 to 9.