Manufacturing method of silicon carbide product and silicon carbide product
By adopting slurry method and multi-layer intermediate film sintering technology, the problem of silicon carbide products being difficult to produce large-area and low-cost in the prior art is solved, and high-strength, corrosion-resistant and high-temperature silicon carbide products are realized. Various application scenarios.
Patent Information
- Application Number
- CN202411295772.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
The existing silicon carbide product production methods are difficult to achieve large area, low cost and high strength at the same time, and large equipment is often required, which increases production costs and technical difficulties.
Using the slurry method, the slurry includes silicon carbide powder, organic binder, inorganic binder, expansion aid and solvent. Through the formation and sintering process of multi-layer intermediate film layers, high-strength large-area silicon carbide products are produced. , avoid the use of large sealing molds and high pressure equipment.
It has achieved low-cost and efficient production of special-shaped structures and large-area silicon carbide products, with high strength, corrosion resistance and high temperature resistance, and is suitable for different application scenarios.
Smart Images

Figure CN119080505A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of silicon carbide, and in particular to a method for manufacturing a silicon carbide product and a silicon carbide product. Background Art
[0002] Silicon carbide has the advantages of corrosion resistance, high temperature resistance, high hardness, good wear resistance, and stable chemical properties. Silicon carbide is usually made into a film layer for different application scenarios. Existing methods for making silicon carbide products usually include powder pressing, extrusion molding, grouting molding, and 3D printing. The above methods are difficult to simultaneously meet the requirements of low production cost and large-area silicon carbide products. Summary of the invention
[0003] In view of this, it is necessary to provide a method for manufacturing a large-area silicon carbide product at a relatively low cost to solve the above problems.
[0004] In the first aspect, the present application provides a method for manufacturing a silicon carbide product, comprising: providing a slurry, the slurry comprising silicon carbide powder, an organic binder, an inorganic binder, an expansion aid and a solvent; forming the slurry on the surface of a mold; baking the mold with the slurry to remove the solvent and thereby form an intermediate film layer; repeating the steps of forming the slurry on the mold and baking at least once to form a multi-layer intermediate film layer; curing the multi-layer intermediate film layer and the mold to form a blank of the multi-layer intermediate film layer, and removing the mold; and sintering the blank in a protective atmosphere to obtain a silicon carbide product.
[0005] In some possible implementations of the present application, the slurry further includes carbon powder, and based on the total mass excluding the solvent, the mass fraction of the carbon powder is W1, and the preparation method satisfies: 2%≤W1≤2%.
[0006] In some possible implementations of the present application, before the sintering step, the manufacturing method further includes: spreading silicon particles on the surface of the embryonic body.
[0007] In some possible embodiments of the present application, the particle size of the silicon carbide powder includes a first particle size and a second particle size, the first particle size is D1, the second particle size is D2, and the manufacturing method satisfies: 8μm≤D1≤20μm, 80μm≤D2≤120μm.
[0008] In some possible embodiments of the present application, based on the total mass excluding the solvent, the mass fraction of the silicon carbide powder of the first particle size is w1, and the production method satisfies: 15%≤w1≤45%; the mass fraction of the silicon carbide powder of the second particle size is w2, and the production method satisfies: 25%≤w2≤55%.
[0009] In some possible embodiments of the present application, based on the total mass excluding the solvent, the mass fraction of the organic binder is W2, and the manufacturing method satisfies: 2%≤W2≤5%; the mass fraction of the inorganic binder is W3, and the manufacturing method satisfies: 6%≤W3≤20%.
[0010] In some possible embodiments of the present application, before the step of forming the slurry on the surface of the mold, the manufacturing method further includes: forming a release layer on the surface of the mold; in the curing step, the release layer forms powder to facilitate separation of the embryo from the mold.
[0011] In some possible implementations of the present application, the temperature of the curing treatment is T, and the manufacturing method satisfies: 180°C≤T≤250°C; the time of the curing treatment is t, and the manufacturing method satisfies: 30min≤t≤60min.
[0012] In a second aspect, the present application also provides a silicon carbide product, which is produced by the above-mentioned production method.
[0013] On the third aspect, the present application also provides a silicon carbide product, which is a hollow tube body. The wall thickness of the silicon carbide product is l1, and the silicon carbide product satisfies: 0.1mm≤l1≤5mm; the length of the silicon carbide product is l2, and the silicon carbide product satisfies: 2m≤l2≤4m; the diameter of the silicon carbide product is l3, and the silicon carbide product satisfies: 0.4m≤l3≤1m.
[0014] The method for manufacturing a silicon carbide product provided in the embodiment of the present application can manufacture silicon carbide products with special-shaped structures and large areas. In addition, the method for manufacturing provided in the embodiment of the present application is easy to operate and low in cost. During the manufacturing process, there is no need to use large sealed molds, high-strength molds, high-pressure equipment (such as die-casting machines), etc. In addition, according to the composition of the slurry and the specific manufacturing steps, high-strength silicon carbide products can be manufactured. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 A flow chart of a method for manufacturing a silicon carbide product provided in an embodiment of the present application. DETAILED DESCRIPTION
[0016] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the present application is described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that, in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other. In the following description, many specific details are set forth to facilitate a full understanding of the present application, and the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments.
[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this article are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes all and any combination of one or more related listed items.
[0018] The steps of making silicon carbide products by powder pressing generally include: using large equipment to press the powder containing silicon carbide to form a blank, and then drying, sintering and other steps to form a silicon carbide product. The above production method has small volume shrinkage and high density; however, the powder has low fluidity, making it difficult to make silicon carbide products with special-shaped structures, and it is difficult to make large-area, thin silicon carbide products. Large equipment is used, and the production cost is high.
[0019] The steps of making silicon carbide products by extrusion molding generally include: extruding a slurry containing silicon carbide to form a blank, and then drying, sintering and other steps to form a silicon carbide product. In the above production method, the fluidity of the slurry is improved compared to the powder, but in the extrusion molding process, it is a one-time molding, the volume shrinkage of the slurry is large, the silicon carbide products produced are prone to cracking, and it is difficult to produce large-area, thinner silicon carbide products; large equipment is also required for production, which increases costs.
[0020] The steps of making silicon carbide products by slip injection molding generally include: injecting slurry containing silicon carbide into a mold to form a blank, and then drying, sintering and other steps to form a silicon carbide product. In the above production method, the fluidity of the slurry is improved compared to the powder, but it is easy to deform during the production process, making it difficult to produce large-area, thin silicon carbide products.
[0021] The steps of making silicon carbide products by 3D printing generally include: 3D printing a slurry containing silicon carbide to form an embryo, followed by drying, sintering and other steps to form a silicon carbide product. The above-mentioned production method has strict requirements on the particle size, shape, material, etc. in the slurry, and has high technical requirements, so the cost is relatively high; and the silicon carbide products made by 3D printing have relatively low strength, and it is difficult to control the quality of silicon carbide products.
[0022] The present application embodiment provides a method for manufacturing a silicon carbide product that can manufacture a large area of silicon carbide products and has relatively low cost. Figure 1 , the preparation method may include the following steps:
[0023] Step S1: providing a slurry, wherein the slurry includes silicon carbide powder, an organic binder, an inorganic binder, an expansion aid and a solvent.
[0024] Based on the total mass excluding the solvent, the mass fraction of silicon carbide powder is W0, and the manufacturing method can satisfy: 40% ≤ W0 ≤ 80%. In some embodiments of the present application, the mass fraction of silicon carbide powder can be 45%, 52%, 56%, 62% or 66%, etc. Silicon carbide powder is the main material for forming silicon carbide products, and the mass fraction of silicon carbide powder is relatively large. It should be noted that the "mass fraction" of the components in the subsequent slurry is based on the total mass excluding the solvent.
[0025] The particle size of silicon carbide powder includes a first particle size and a second particle size, the first particle size is D1, the second particle size is D2, and the manufacturing method can satisfy: 8μm≤D1≤20μm, 80μm≤D2≤120μm. In some embodiments of the present application, the first particle size can be 10μm, 13μm, 15μm or 18μm, etc., and the second particle size can be 85μm, 92μm, 96μm, 105μm, 112μm or 118μm, etc. Silicon carbide powders of different particle size ranges are set, and silicon carbide powders with smaller particle sizes can be filled between silicon carbide powders with larger particle sizes, thereby increasing the density of the slurry, which is beneficial to improve the cracking problem during the subsequent curing or sintering process. In some embodiments, the numerical value of the second particle size is 7 to 10 times the numerical value of the first particle size, and silicon carbide of the first particle size can fully fill the gaps between silicon carbide of the second particle size. If the first particle size of silicon carbide is too small or too large, it is difficult for silicon carbide of the first particle size to fully fill the gaps between silicon carbide of the second particle size, resulting in a decrease in the strength of the silicon carbide product formed subsequently. If the second particle size of silicon carbide is too small, the gaps between silicon carbide of the second particle size are small, and it is difficult for silicon carbide of the first particle size to fully fill the gaps, resulting in a decrease in the strength of the silicon carbide product formed subsequently; if the second particle size of silicon carbide is too large, similarly, it will affect the decrease in the strength of the silicon carbide product, and at the same time, the surface of the silicon carbide product obtained will be rough, further affecting the strength of the silicon carbide product.
[0026] The mass fraction of the silicon carbide powder of the first particle size is w1, and the production method can satisfy: 15% ≤ w1 ≤ 45%; the mass fraction of the silicon carbide powder of the second particle size is w2, and the production method can satisfy: 25% ≤ w2 ≤ 55%. In some embodiments of the present application, the mass fraction range of the silicon carbide powder of the first particle size can be 20%, 24%, 28%, 32% or 36%, etc., and the mass fraction range of the silicon carbide powder of the second particle size can be 27%, 32%, 35%, 42% or 48%, etc.
[0027] The organic binder can be selected from at least one of phenolic resin, epoxy resin, polyester resin and alkyd resin. The inorganic binder can be selected from at least one of silica sol, aluminum sol, phosphate and water glass. The organic binder is used to increase the viscosity of the slurry, wherein, in the subsequent slurry coating, embryo body formation, low temperature sintering stage and other processes, it plays a bonding role, which is beneficial to increase the strength of the embryo body; in the subsequent sintering process in a protective atmosphere, the molecular chain in the organic binder breaks and decomposes into low molecular weight substances, and the non-carbon elements (such as hydrogen, oxygen, nitrogen, etc.) in the organic binder gradually volatilize in the form of gas, such as NH3, N2, H2O, etc., and the carbon element forms carbon powder, and the carbon atoms in the carbon powder can combine with silicon atoms to form carbon-silicon bonds, thereby forming an integrated structure connected by chemical bonds to increase the strength of the formed silicon carbide product; the inorganic binder plays a bonding role in the subsequent slurry coating, embryo body formation, high temperature sintering stage and the formed silicon carbide product.
[0028] The mass fraction of the organic binder is W2, and the manufacturing method can satisfy: 2% ≤ W2 ≤ 5%. In some embodiments of the present application, the mass fraction of the organic binder can be 2.5%, 2.8%, 3.5% or 4.2%, etc. If the mass fraction of the organic binder is too small, it is difficult to play a bonding role, and in the subsequent coating process of the slurry, the coated slurry is difficult to shape; if the mass fraction of the organic binder is too large, the viscosity of the slurry is too large, and the slurry is difficult to coat evenly. The mass fraction of the organic binder is within an appropriate range, which can play a more appropriate bonding role and is conducive to subsequent coating and molding.
[0029] The mass fraction of the inorganic binder is W3, and the manufacturing method can meet the following conditions: 6% ≤ W3 ≤ 20%. In some embodiments of the present application, the mass fraction of the inorganic binder can be 6.5%, 8.8%, 10.5%, 12.5%, 15.5%, 16.8% or 18.2%, etc. If the mass fraction of the inorganic binder is too small, it is difficult to play a bonding role, especially after high-temperature sintering and carbonization of the organic binder and loss of bonding effect, which can easily lead to cracking of the embryo formed after sintering; if the mass fraction of the inorganic binder is too large, the silicon carbide product obtained will have more inorganic binder, which will affect the performance of the silicon carbide product.
[0030] The mass fraction of the expansion aid is W4, and the manufacturing method can satisfy: 4%≤W4≤8%. In some embodiments of the present application, the mass fraction of the expansion aid can be 4.5%, 5.8%, 6.5% or 7.2%, etc. The expansion aid can be selected from at least one of zirconium oxide, magnesium oxide, titanium oxide and aluminum oxide. The expansion aid is used to bring about volume expansion in different temperature ranges, such as 100°C to 200°C, 350°C to 450°C, etc. In the subsequent processing of the slurry, there will be volume shrinkage caused by solvent volatilization, cross-linking reaction or decomposition and volatilization of organic binders during the sintering process, resulting in various stresses inside the material. The expansion aid can alleviate these stresses to a certain extent through expansion, reduce the risk of cracking caused by stress concentration, and thus improve the problem of cracking of the slurry in subsequent processing.
[0031] The balance in the slurry is a solvent, which may be water, and the components in the slurry may be dissolved or dispersed in the solvent.
[0032] In some embodiments of the present application, the slurry may also contain carbon powder, the mass fraction of the carbon powder is W1, the preparation method may satisfy: 2% ≤ W1 ≤ 5%, and the particle size range of the carbon powder may be 0.5 μm-1 μm. In some embodiments, the mass fraction of the carbon powder may be 2.4%, 2.8%, 3.6% or 4.5%, etc., and the particle size of the carbon powder may be 2.4 μm, 3.2 μm, 3.8 μm or 4.5 μm, etc. The carbon powder formed after carbonization of the carbon powder and the organic binder is used in the subsequent sintering process to react with the silicon element to form an integrated structure to increase the strength of the formed silicon carbide product.
[0033] Step S2: forming a release layer on the surface of the mold.
[0034] The material of the mold can be quartz glass, polypropylene, polytetrafluoroethylene or metal, etc. The shape of the mold is set according to the shape of the silicon carbide product to be formed. In this embodiment, the shape of the mold is tubular.
[0035] The demoulding layer is formed on the surface of the mold, and the demoulding layer facilitates the subsequent demoulding process. The demoulding layer can be selected from a resin with lower high temperature resistance than the mold, such as epoxy resin, unsaturated alkyd resin, etc., or can be selected from demoulding wax, demoulding paste, vaseline, etc.
[0036] Step S3: forming the slurry on the surface of the mold with the release layer.
[0037] The slurry is sprayed on the surface of the mold provided with the release layer. The thickness of the slurry sprayed on the mold is set according to the required thickness of the silicon carbide product. In some embodiments, the thickness of the slurry provided on the mold can be between 0.2 mm and 1 mm. Since the slurry is viscous, the slurry can adhere to the surface of the mold.
[0038] Step S4: baking the mold with the slurry to remove the solvent, thereby forming an intermediate film layer.
[0039] In this embodiment, the solvent is water, the baking temperature can be 60° C.-90° C., and the baking time is 10 min-120 min. In other embodiments, the baking temperature can be adjusted according to different types of solvents.
[0040] The thickness of the intermediate film layer formed after the solvent is removed will shrink to a certain extent relative to the thickness of the slurry formed on the mold surface before the baking treatment.
[0041] Repeat step S3 and step S4 at least once, that is, repeat the steps of forming slurry on the mold and baking at least once to form a multi-layer intermediate film layer, which is equivalent to increasing the thickness of the intermediate film layer. According to the actual thickness requirements, the number of times to repeat step S3 and step S4 is selected. Among them, in this embodiment, the thickness of the silicon carbide product to be produced is 2mm-3mm, and the number of times to repeat step S3 and step S4 is selected. Compared with completing the coating amount in one time, this embodiment adopts a method of multiple coatings and drying treatments, which can remove the solvent in advance to eliminate most of the shrinkage, which is beneficial to improve the cracking problem caused by the shrinkage of the intermediate film layer after removing the solvent; in addition, even if cracking occurs, in the subsequent step of coating the slurry, the slurry can fill the cracked area to improve the cracking problem.
[0042] Step S5: curing the intermediate film layer and the mold that have been repeatedly formed to form an embryonic body, and removing the mold.
[0043] The middle film layer covered with the mold is placed in an oven for curing treatment. The curing temperature is T, and the manufacturing method can meet the following conditions: 180℃≤T≤250℃. The curing time is t, and the manufacturing method meets the following conditions: 30min≤t≤60min. The middle film layer further removes the solvent in the oven. In addition, the organic binder and the inorganic binder undergo a cross-linking reaction during the curing process, so that the middle film layer forms a hard embryo. In the curing process, the evaporation of the solvent will bring about a certain volume change. The expansion aid expands due to heat at this time, which can compensate for the volume change caused by the evaporation of the solvent to prevent the embryo from cracking.
[0044] The high temperature resistance of the demoulding layer is lower than that of the mold. During the curing process, the demoulding layer softens or carbonizes to form powder, and the mold can still maintain its original shape. A gap is formed between the embryo and the mold to facilitate separation of the embryo and the mold.
[0045] Step S6: sintering the embryo in a protective atmosphere to obtain a silicon carbide product.
[0046] During the sintering process, at a temperature range of about 350°C-450°C, the organic binder in the embryo will carbonize and cause a volume change. During this process, the expansion aid will expand due to the heat, which can compensate for the volume change caused by the carbonization of the organic binder to prevent the embryo from cracking.
[0047] Sintering is carried out in an argon atmosphere to obtain silicon carbide powder. During the sintering process, a gradual heating method is used for sintering, that is, multiple stages of heating and heat preservation steps are included to prevent the temperature from rising too fast and causing cracking of the embryo. In some embodiments, the specific heating steps may include: heating from room temperature to 800°C, taking 80min-160min, and keeping warm for 30min-60min; heating from 800°C to 1000°C, taking 30min-60min, and keeping warm for 20min-40min; heating from 1000°C to 1200°C, taking 40min-60min, and keeping warm for 60-90min; heating from 1200°C to 1400°C, taking 40min-60min, and keeping warm for 120min-240min; heating from 1400°C to 1730°C, taking 40min-80min, and keeping warm for 90min-180min.
[0048] Before the sintering step, the manufacturing method also includes laying silicon particles on the surface of the embryo. During the sintering process, liquid silicon is formed after about 1400°C, and the liquid silicon penetrates into the embryo and chemically reacts with the carbon element in the embryo to form silicon carbide, thereby forming an integrated structure. Among them, the carbon element includes the carbon element in the carbon powder and the carbon element in the silicon carbide powder. The carbon powder includes the carbon powder added to the slurry and the carbonized organic binder to form the carbon powder. The carbon powder will also chemically react with the silicon element in the silicon carbide powder to form silicon carbide, thereby forming a tight integrated structure.
[0049] In some embodiments, the mass of silicon particles laid on the surface of the embryo can be 0.6 to 1.2 times the mass of the embryo, which ensures that the liquid silicon formed during the sintering process is more than the liquid silicon that can be absorbed by the embryo, and avoids waste due to excessive silicon particles and the workload of subsequent silicon particle removal.
[0050] After the sintering step is completed, the cooling is carried out in a gradual cooling manner, that is, including multi-stage cooling and heat preservation steps, to prevent the temperature from cooling too fast and causing cracking of the silicon carbide product. In some embodiments, the specific heating step may include: cooling from 1730°C to 1300°C, which takes 80min-150min; cooling from 1300°C to room temperature, which takes 250min-300min.
[0051] The manufacturing method may also include grinding the silicon carbide product to remove excess silicon particles and burrs so as to produce a finished product.
[0052] In this embodiment, the shape of the mold is tubular, the shape of the formed embryo is a hollow tube, and the silicon carbide product obtained after sintering is also a hollow tube. In other embodiments, the shape of the mold can be changed according to the shape to be formed to obtain silicon carbide products of other shapes, such as silicon carbide products in sheet, arc, special shape, etc.
[0053] Through the manufacturing method provided in the embodiment of the present application, it is possible to manufacture special-shaped structures and large-area (e.g. 5m 2 -20m 2 In addition, the manufacturing method provided in the embodiment of the present application is easy to operate and has low cost. During the manufacturing process, there is no need to use large sealed molds, high-strength molds, high-pressure equipment (such as die-casting machines), etc. In addition, according to the composition of the slurry and the specific manufacturing steps, high-strength silicon carbide products can be manufactured.
[0054] Silicon carbide products have the advantages of corrosion resistance, high temperature resistance, high hardness, good wear resistance, and stable chemical properties. They can be used in different scenarios according to the shape of the silicon carbide products, such as in the preparation of equipment in the semiconductor and photovoltaic fields, high temperature and corrosion resistant equipment, etc.
[0055] In some embodiments, a silicon carbide product made by the above-mentioned manufacturing method is provided, wherein the silicon carbide product is a tube body with a hollow interior, and the wall thickness of the silicon carbide product is l1, and the silicon carbide product can satisfy: 0.1mm≤l1≤5mm; the length of the silicon carbide product is l2, and the silicon carbide product can satisfy: 2m≤l2≤4m; the diameter of the silicon carbide product is l3, and the silicon carbide product can satisfy: 0.4m≤l3≤1m. The tubular silicon carbide product can be used as a conveying pipe and a high-temperature heating pipe.
[0056] In some embodiments, the silicon carbide product can be fabricated into a corrosion-resistant reaction container, such as a beaker.
[0057] The following describes the method for manufacturing the silicon carbide product provided in the present application through specific examples and comparative examples.
[0058] Example 1-1
[0059] A slurry is provided, which includes silicon carbide powder, an organic binder, an inorganic binder, an expansion aid, carbon powder and a solvent. The silicon carbide powder has two different particle size ranges, the mass fraction of the silicon carbide powder of the first particle size is 25%, and the mass fraction of the silicon carbide powder of the second particle size is 45%; the organic binder is a phenolic resin, the mass fraction of the phenolic resin is 3%; the inorganic binder is a silica sol, the mass fraction of the silica sol is 15%; the expansion aid is zirconium oxide, the mass fraction of zirconium oxide is 5%; the mass fraction of carbon powder is 8%; and the solvent is water.
[0060] The slurry is formed on the surface of the mold with the release layer, and the mold with the slurry is baked to remove the solvent, thereby forming an intermediate film layer. The step of forming the intermediate film layer is repeated 3 times, that is, the number of times of forming the intermediate film layer is carried out 4 times in total. The intermediate film layer and the mold formed after multiple repetitions are cured to form an embryonic body of the intermediate film layer, and the mold is removed.
[0061] The embryo is sintered in an argon atmosphere to obtain a silicon carbide product. The specific heating steps include: heating from room temperature to 800°C for 120 minutes and keeping warm for 40 minutes; heating from 800°C to 1000°C for 40 minutes and keeping warm for 30 minutes; heating from 1000°C to 1200°C for 50 minutes and keeping warm for 70 minutes; heating from 1200°C to 1400°C for 50 minutes and keeping warm for 180 minutes; heating from 1400°C to 1730°C for 60 minutes and keeping warm for 120 minutes.
[0062] The silicon carbide product is subjected to performance testing, which includes testing the embryo strength, cooked embryo density and observing the embryo cracking. Among them, embryo strength refers to the ability of the embryo to resist damage under the action of external force. The higher the embryo strength, the more effective it is to prevent the embryo from cracking during subsequent sintering and transportation. Cooked embryo density refers to the density of the silicon carbide product. The higher the cooked embryo density, the more sophisticated the silicon carbide product is, which is beneficial to improving the extrusion resistance, acid and alkali resistance, etc. of the silicon carbide product. The initial embryo strength of the silicon carbide product produced in this embodiment is 15MP, and the cooked embryo density is 2.8g / cm 3 .
[0063] Example 1-2
[0064] The difference from Example 1-1 is that the organic binder in Example 1-2 is epoxy resin. The silicon carbide product produced in Example 1-2 has a body strength of 13MP and a cooked body density of 2.7g / cm 3 .
[0065] Examples 1-3
[0066] The difference from Example 1-1 is that the organic binder in Example 1-3 is polyaldehyde resin. The silicon carbide product produced in Example 1-3 has a body strength of 12MP and a cooked body density of 2.65g / cm 3 .
[0067] The following are examples 1-1 to 1-3 summarized, and the specific results are shown in Table 1.
[0068] Table 1
[0069]
[0070]
[0071] From the test results in Table 1, it can be seen that phenolic resin, epoxy resin and polyester resin can all be used as organic binders, and can all be made into silicon carbide products with suitable embryo strength and cooked embryo density. Among them, when phenolic resin is used as an organic binder, the embryo strength is relatively high, the cooked embryo density is relatively high, and the performance is better.
[0072] The specific steps of Example 2-1, Example 2-2 and Example 2-3 can refer to Example 1-1, wherein Table 2 lists the relevant parameters and corresponding test structures of Example 2-1, Example 2-2 and Example 2-3.
[0073] Table 2
[0074]
[0075] It can be seen from the test structure in Table 2 that the particle size of silicon carbide powder has a certain influence on the embryo strength and the cooked embryo density. When the mass fraction of silicon carbide powder of the first particle size is 15%≤w1≤45% and the mass fraction of silicon carbide powder of the second particle size is 25%≤w1≤55%, silicon carbide products with suitable embryo strength and cooked embryo density can be obtained. Among them, when the mass fraction of the first particle size is 25% and the mass fraction of the second particle size is 45% in Example 2-3, the silicon carbide powder of the first particle size can be fully dispersed in the silicon carbide powder of the second particle size, and the performance of the obtained silicon carbide product is relatively good.
[0076] The specific steps of Example 3-1, Example 3-2 and Example 3-3 can refer to Example 1-1, wherein Table 3 lists the relevant parameters and corresponding test structures of Example 3-1, Example 3-2 and Example 3-3.
[0077] Table 3
[0078]
[0079]
[0080] From the test structure in Table 3, it can be seen that the mass fraction of carbon powder in the slurry has a certain influence on the performance of the silicon carbide product. During the sintering process, the carbon atoms and silicon atoms in the carbon powder can combine with each other to form carbon-silicon bonds, thereby forming an integrated structure connected by chemical bonds to increase the strength of the formed silicon carbide product. Among them, when the mass fraction of carbon powder in Example 3-1 is 7%, the embryo strength is relatively high, the cooked embryo density is relatively high, and the performance is better.
[0081] The specific steps of Example 4-1, Example 4-2 and Example 4-3 can refer to Example 1-1, wherein Table 4 lists the relevant parameters and corresponding test structures of Example 4-1, Example 4-2 and Example 4-3.
[0082] Table 4
[0083]
[0084] From the test structure in Table 4, it can be seen that the mass fraction of the organic binder has a certain influence on the performance of the silicon carbide product. When the mass fraction of the phenolic resin is 3%, the performance of the silicon carbide product is better.
[0085] The specific steps of Example 5-1, Example 5-2, Example 5-3 and Comparative Example 1 can refer to Example 1-1, wherein Table 5 lists the relevant parameters of Example 5-1, Example 5-2, Example 5-3 and Comparative Example 1 and the corresponding test structures.
[0086] Table 5
[0087]
[0088]
[0089] It can be seen from the test structure in Table 5 that in the step of making silicon carbide products, an expansion aid is added to the slurry to compensate for the volume shrinkage caused by solvent volatilization, cross-linking reaction or decomposition and volatilization of organic binders during sintering, thereby improving the problem of cracking of the slurry in subsequent processing. Among them, zirconium oxide, magnesium oxide, and aluminum oxide can all be used as expansion aids. When zirconium oxide is used as an expansion aid, the anti-cracking performance of the embryo is better.
[0090] The specific steps of Example 6-1, Example 6-2 and Example 6-3 can refer to Example 1-1, wherein Table 6 lists the relevant parameters and corresponding test structures of Example 6-1, Example 6-2 and Example 6-3.
[0091] Table 6
[0092]
[0093] From the test structure in Table 6, it can be seen that the mass fraction of the expansion aid has a certain influence on the performance of the silicon carbide product. When the mass fraction of zirconium oxide is 5%, the performance of the silicon carbide product is better.
[0094] The specific steps of Example 7-1, Example 7-2, Example 7-3 and Comparative Example 2 can refer to Example 1-1, wherein Table 7 lists the relevant parameters of Example 7-1, Example 7-2, Example 7-3 and Comparative Example 2 and the corresponding test structures.
[0095] Table 7
[0096]
[0097]
[0098] From the test structure in Table 7, it can be seen that the inorganic binder can play a bonding role in the slurry coating, embryo body formation, high-temperature sintering stage and the formed silicon carbide product. When the inorganic binder is not added to the slurry, the embryo body will crack seriously. Among them, since the organic binder will be carbonized to form carbon powder in the protective atmosphere during the high-temperature sintering process, the organic binder loses its bonding effect, but the inorganic binder can still play a bonding role, which is conducive to improving the embryo body cracking phenomenon during the high-temperature sintering process.
[0099] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A method for producing a silicon carbide product, characterized in that: include: Providing a slurry, wherein the slurry includes silicon carbide powder, an organic binder, an inorganic binder, an expansion aid and a solvent; forming the slurry on the surface of a mold; Baking the mold with the slurry to remove the solvent and form an intermediate film layer; Repeating the steps of forming the slurry on the mold and baking at least once to form multiple layers of the intermediate film layer; Curing the multiple layers of the intermediate film layers and the mold to form an embryonic body, and removing the mold; as well as The green body is sintered in a protective atmosphere to obtain the silicon carbide product.
2. The method for manufacturing a silicon carbide product according to claim 1, characterized in that: The slurry further comprises carbon powder. Based on the total mass excluding the solvent, the mass fraction of the carbon powder is W1. The preparation method satisfies: 2%≤W1≤2%.
3. The method for manufacturing a silicon carbide product according to claim 1, characterized in that: Before the sintering step, the manufacturing method further comprises: spreading silicon particles on the surface of the embryonic body.
4. The method for manufacturing a silicon carbide product according to claim 1, characterized in that: The particle size of the silicon carbide powder includes a first particle size and a second particle size, the first particle size is D1, the second particle size is D2, and the manufacturing method satisfies: 8μm≤D1≤20μm, 80μm≤D2≤120μm.
5. The method for manufacturing a silicon carbide product according to claim 4, characterized in that: Based on the total mass excluding the solvent, the mass fraction of the silicon carbide powder of the first particle size is w1, and the production method satisfies: 15%≤w1≤45%; the mass fraction of the silicon carbide powder of the second particle size is w2, and the production method satisfies: 25%≤w2≤55%.
6. The method for manufacturing a silicon carbide product according to claim 1, characterized in that: Based on the total mass excluding the solvent, the mass fraction of the organic binder is W2, and the preparation method satisfies: 2%≤W2≤5%; the mass fraction of the inorganic binder is W3, and the preparation method satisfies: 6%≤W3≤20%.
7. The method for manufacturing a silicon carbide product according to claim 1, characterized in that: Before the step of forming the slurry on the surface of the mold, the manufacturing method further comprises: forming a release layer on the surface of the mold; In the curing process, the demoulding layer is formed into powder, so as to facilitate the separation of the embryo body from the mold.
8. The method for manufacturing a silicon carbide product according to claim 1, characterized in that: The temperature of the curing treatment is T, and the manufacturing method satisfies: 180°C≤T≤250°C; the time of the curing treatment is t, and the manufacturing method satisfies: 30min≤t≤60min.
9. A silicon carbide product, characterized in that: The invention is prepared by the preparation method described in any one of claims 1 to 8.
10. A silicon carbide product, characterized in that: The silicon carbide product is a hollow tube body, the wall thickness of the silicon carbide product is l1, and the silicon carbide product satisfies: 0.1mm≤l1≤5mm; the length of the silicon carbide product is l2, and the silicon carbide product satisfies: 2m≤l2≤4m; the diameter of the silicon carbide product is l3, and the silicon carbide product satisfies: 0.4m≤l3≤1m.
Citation Information
Patent Citations
Preparation method of pure silicon carbide porous ceramic membrane
CN104261867A
Pipeline or pipe fitting provided with silicon carbide ceramic abrasion-resisting and corrosion-resisting liner and preparation method thereof
CN106917918A
Forming method adopting infiltration method to make reactive sintering silicon carbide ceramic and die
CN107827466A
Reaction sintering silicon carbide ceramic and preparation method thereof
CN114956831A
Reaction sintering silicon carbide and wet forming preparation method thereof
CN116425550A
Cited By
A double system forming compound for complex shape silicon carbide ceramics and its preparation method
CN122809897A