Sintering method based on sintering temperature curve of high-porosity honeycomb ceramic
By controlling the firing temperature curve and heat transfer method of high porosity honeycomb ceramics, the problems of low yield and cracking of finished products during the sintering process of honeycomb ceramics in the prior art are solved, and high-quality firing and heat transfer efficiency are achieved.
Patent Information
- Application Number
- CN202411249876.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high porosity and small pore size honeycomb ceramics have low yields due to rapid heating during sintering, and the heat transfer method has problems such as too high temperature or too large temperature difference, resulting in product cracking.
The sintering temperature curve method based on high porosity honeycomb ceramics is adopted, and the optimal sintering coking discharge speed is determined through multiple steps of heating and cooling control. Combined with the heat transfer method of hot air circulation and heat radiation, the sintering coking is smoothly discharged, and the temperature difference between the upper and lower is controlled. Avoid intense combustion and degreasing incomplete completion, ensuring that the product is synchronously coking and molding.
The performance technical parameters and pass rate of the product are improved, cracking is avoided, and efficient heat transfer and high-quality molding of the finished product are achieved.
Smart Images

Figure CN119080513A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of honeycomb ceramics, and in particular to a sintering method based on a sintering temperature curve of high-porosity honeycomb ceramics. Background Art
[0002] The development of the industrialization of the automobile industry has brought about increasingly serious exhaust pollution. As the control standards for automobile exhaust emissions become increasingly stringent, countries around the world, including China, are also increasingly tightening their control over diesel vehicle exhaust emissions.
[0003] The raw materials of small-pore and high-porosity products are relatively fine, and the pore-forming agent is also fine and large in quantity, which is bound to generate a lot of heat during the product sintering and coking process. When the existing tunnel kiln sinters high-porosity and small-pore honeycomb ceramics, most of them adopt rapid sintering, especially in the coking section, a faster heating rate is still adopted. Although this sintering method is more efficient, the yield rate of the finished product is average, and hot air circulation is used in the coking section or the heat of the insulation section is pumped to the coking section. The heat transfer method is mainly thermal radiation. Both have defects. The former has too high temperature and fierce degreasing; the latter has a high temperature difference between the upper and lower sections in the same section, and cannot be coked synchronously, resulting in product cracking. Summary of the invention
[0004] Purpose of the invention:
[0005] In order to overcome the problems existing in the prior art, the present invention provides a firing method based on the firing temperature curve of high-porosity honeycomb ceramics. The optimal firing and coking speed is determined according to the combustion temperatures of various pore-forming agents through research, and the upper and lower temperature differences are controlled in this section to improve the heat transfer efficiency, so that the coking of products in the same section is synchronized, and the coking is smoothly discharged according to the set temperature curve to avoid cracking caused by violent combustion or incomplete degreasing. Finally, the entire firing curve is determined according to the performance requirements of the product to achieve the performance technical parameters of the fired product and a high product qualification rate.
[0006] In order to solve the above problems, the present invention adopts the following technical solutions:
[0007] A sintering method based on a sintering temperature curve of a high-porosity honeycomb ceramic comprises the following steps:
[0008] S1. Heating the temperature from room temperature to 250°C at a rate of 9°C / hour to dry the clay embryo and discharge free water so that the moisture content of the clay embryo is less than 0.5%;
[0009] S2. The temperature is raised from 250°C to 400°C at a rate of 4°C / hour, and the organic binder and pore former are discharged successively. The coke discharge speed is slowed down to prevent the organic matter and pore former from burning violently and cracking;
[0010] S3, heating from 400°C to 800°C at a rate of 8°C / hour to dehydrate the raw materials, prevent the discharge of organic matter and water together, and control cracking;
[0011] S4, heating from 800°C to 1250°C at a rate of 8°C / hour, solid phase reaction, rapid heating to prevent the diffusion of magnesium aluminum spinel produced by talc decomposition and affect the pore size distribution;
[0012] S5, heating from 1250°C to 1420°C at a rate of 3°C / hour, high temperature liquid phase reaction, slowing down the heating rate, and fully precipitating cordierite crystals;
[0013] S6, maintain 1420℃ for 8 hours, fully keep warm, so that the cordierite reacts completely and the crystal grows completely;
[0014] S7, cooling down from 1420℃ to 1200℃ at a rate of 40℃ / hour, rapid cooling to form micro cracks, and improving the thermal shock resistance of the product;
[0015] S8. Cool down from 1200°C to room temperature at a rate of 13°C / hour, let stand to cool, and the product is formed.
[0016] Preferably, in steps S1 to S8, the clay embryo is placed in a tunnel kiln for sintering.
[0017] Preferably, in step S1, microwave drying and hot air drying are used for drying the clay embryo until the moisture content is less than 0.5%, and then hot air with a moisture content of 0.5% is used instead.
[0018] Preferably, in step S2, the heat transfer method adopts hot air circulation and heat radiation, and both are carried out simultaneously to control the upper and lower temperature difference within 10° C., and the heat exchange is carried out evenly.
[0019] Preferably, the hot air circulation method is to heat the coke discharge section in the form of hot air using the heat generated by the combustion of the organic gas after coke discharge in the incinerator, and at the same time, the stirring air is injected into the kiln after heat exchange to form an air vortex, so that the heat can be retained.
[0020] Preferably, the heat radiation method is to use 50°C induced wind at the tunnel kiln head entrance to form a wind wall, so that the tunnel kiln head maintains a slightly positive pressure, and uses traction wind to bring the high temperature heat of the insulation section to the coke discharge section, and conduct it in the form of heat radiation.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0022] 1. Through research, the optimal firing and coking speed is determined according to the combustion temperature of various pore-forming agents, and the coking is smoothly discharged according to the set temperature curve to avoid cracking caused by violent combustion or incomplete degreasing. Finally, the entire firing curve is determined according to the performance requirements of the product to achieve the performance technical parameters and high product qualification rate of the fired product.
[0023] 2. In step S2, the heat transfer method adopts hot air circulation and heat radiation, and both are carried out simultaneously to control the upper and lower temperature difference within 10°C, the heat exchange is carried out evenly, and the glue is removed synchronously, which further improves the product qualification rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of temperature rise discount of the present invention;
[0025] Figure 2 It is a schematic diagram of the temperature rise discount of the prior art; DETAILED DESCRIPTION
[0026] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0027] Any feature disclosed in this specification (including any additional claims, abstract and drawings), unless otherwise stated, may be replaced by other alternative features that are equivalent or have similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0029] Example
[0030] like Figure 1 As shown, a sintering method based on a sintering temperature curve of a high porosity honeycomb ceramic comprises the following steps:
[0031] S1. The temperature is raised from room temperature to 250°C at a rate of 9°C / hour, and the clay embryo is dried by microwave drying and hot air drying to discharge free water so that the moisture content of the clay embryo is less than 0.5%, and hot air with a moisture content of 0.5% is used instead;
[0032] S2. The temperature is raised from 250°C to 400°C at a heating rate of 4°C / hour, and the organic binder and pore-forming agent are discharged successively. The coke discharge speed is slowed down to prevent the organic matter and pore-forming agent from burning violently and cracking. A 50°C induced wind is used at the kiln head entrance to form a wind wall to keep a slightly positive pressure at the tunnel kiln head. The heat transfer method of the coke discharge section is hot air circulation and thermal radiation. The heat generated by the combustion of the organic gas after coke discharge in the incinerator is used to heat the coke discharge section in the form of hot air. At the same time, the stirring air is injected into the kiln after heat exchange to form an air vortex, and the heat is retained. At the same time, the high-temperature heat of the insulation section is brought to the coke discharge section by traction wind and conducted in the form of thermal radiation. The simultaneous operation of the two can control the temperature difference between the upper and lower sections within 10°C and ensure uniform heat exchange.
[0033] S3, heating from 400°C to 800°C at a rate of 8°C / hour to dehydrate the raw materials, prevent the discharge of organic matter and water together, and control cracking;
[0034] S4, heating from 800°C to 1250°C at a rate of 8°C / hour, solid phase reaction, rapid heating to prevent the diffusion of magnesium aluminum spinel produced by talc decomposition and affect the pore size distribution;
[0035] S5, heating from 1250°C to 1420°C at a rate of 3°C / hour, high temperature liquid phase reaction, slowing down the heating rate, and fully precipitating cordierite crystals;
[0036] S6, maintain 1420℃ for 8 hours, fully keep warm, so that the cordierite reacts completely and the crystal grows completely;
[0037] S7, cooling down from 1420℃ to 1200℃ at a rate of 40℃ / hour, rapid cooling to form micro cracks, and improving the thermal shock resistance of the product;
[0038] S8. Cool down from 1200°C to room temperature at a rate of 13°C / hour, let stand to cool, and the product is formed.
[0039] In steps S1 to S8, the clay embryo is placed in a tunnel kiln for sintering.
[0040] The overall time of the embodiment is 322 hours, and the product yield reaches 98%.
[0041] Comparative Example
[0042] like Figure 2 As shown, a method for sintering a high-porosity honeycomb ceramic comprises the following steps:
[0043] S1, heating from room temperature to 200°C at a rate of 10°C / hour;
[0044] S2, heating from 200°C to 400°C at a heating rate of 8°C / hour;
[0045] S3, heating from 400°C to 1450°C at a heating rate of 8°C / hour;
[0046] S4, 1450℃, maintain for 8 hours, fully keep warm, so that the cordierite reacts completely and the crystals grow completely;
[0047] S5. Cool down from 1420 to room temperature at a rate of 45°C / hour.
[0048] The overall time of the embodiment is 205 hours, and the product yield is 78%.
[0049] The purpose of the above embodiments is to exemplarily reproduce and deduce the technical solution of the present invention, and to fully describe the technical solution, purpose and effect of the present invention. Its purpose is to make the public understand the disclosed content of the present invention more thoroughly and comprehensively, and it does not limit the scope of protection of the present invention.
[0050] The above embodiments are not exhaustive enumerations of the present invention, and there may be multiple other implementations not listed. Any replacement and improvement made without violating the concept of the present invention shall fall within the protection scope of the present invention.
Claims
1. A sintering method based on a sintering temperature curve of a high porosity honeycomb ceramic, characterized in that: The following steps are involved: S1. Heating the temperature from room temperature to 250°C at a rate of 9°C / hour to dry the clay embryo and discharge free water so that the moisture content of the clay embryo is less than 0.5%; S2. The temperature is raised from 250°C to 400°C at a rate of 4°C / hour, and the organic binder and pore former are discharged successively. The coke discharge speed is slowed down to prevent the organic matter and pore former from burning violently and cracking; S3, heating from 400°C to 800°C at a rate of 8°C / hour to dehydrate the raw materials, prevent the discharge of organic matter and water together, and control cracking; S4, heating from 800°C to 1250°C at a rate of 8°C / hour, solid phase reaction, rapid heating to prevent the diffusion of magnesium aluminum spinel produced by talc decomposition and affect the pore size distribution; S5, heating from 1250°C to 1420°C at a rate of 3°C / hour, high temperature liquid phase reaction, slowing down the heating rate, and fully precipitating cordierite crystals; S6, maintain 1420℃ for 8 hours, fully keep warm, so that the cordierite reacts completely and the crystal grows completely; S7, cooling down from 1420℃ to 1200℃ at a rate of 40℃ / hour, rapid cooling to form micro cracks, and improving the thermal shock resistance of the product; S8. Cool down from 1200°C to room temperature at a rate of 13°C / hour, let stand to cool, and the product is formed.
2. The sintering method based on the sintering temperature curve of high porosity honeycomb ceramics according to claim 1, characterized in that: In steps S1 to S8, the clay embryo is placed in a tunnel kiln for sintering.
3. The sintering method based on the sintering temperature curve of high porosity honeycomb ceramics according to claim 1, characterized in that: In step S1, microwave drying and hot air drying are used to dry the clay embryo until the moisture content is less than 0.5%, and then hot air with a moisture content of 0.5% is used instead.
4. The sintering method based on the sintering temperature curve of high porosity honeycomb ceramics according to claim 1, characterized in that: In step S2, the heat transfer method adopts hot air circulation and heat radiation, and the two are carried out simultaneously to control the upper and lower temperature difference within 10°C, and the heat exchange is carried out evenly.
5. The sintering method based on the sintering temperature curve of high porosity honeycomb ceramics according to claim 4, characterized in that: The hot air circulation method is to heat the coke discharge section in the form of hot air using the heat generated by the combustion of the organic gas after coke discharge in the incinerator. At the same time, the stirring air is injected into the kiln after heat exchange to form an air vortex, so that the heat can be retained.
6. A sintering method based on a sintering temperature curve of a high porosity honeycomb ceramic according to claim 4, characterized in that: The method of heat radiation is to use 50℃ induced wind at the kiln head entrance of the tunnel kiln to form a wind wall, so that the kiln head of the tunnel kiln maintains a slight positive pressure, and use traction wind to bring the high temperature heat from the insulation section to the coke discharge section, and conduct it in the form of heat radiation.