Application of catalyst in preparation of primary amine by catalyzing nitrile compound hydrogenation

By forming a tungsten oxide, molybdenum oxide or vanadium oxide coating on the surface of nickel nanoparticles, the problems of catalyst selectivity and reaction conditions are solved, and efficient and stable hydrogenation reaction of nitrile compounds is achieved, which is suitable for industrial applications. .

CN119080623APending Publication Date: 2024-12-06TAN KAH KEE INNOVATION LAB +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411369538.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing catalysts have low selectivity in the hydrogenation reaction of nitrile compounds, excessive by-products, harsh reaction conditions, and the use of ammonia limits its industrial application prospects.

Method used

By forming a cladding layer of tungsten oxide, molybdenum oxide or vanadium oxide on the surface of nickel nanoparticles, forming a B acid site, improving the selectivity and activity of the catalyst, reducing the amount of ammonia water used, and suitable for catalyzing nitriles under mild conditions. Hydrogenation reaction of compounds.

Benefits of technology

The hydrogenation reaction of nitrile compounds under mild conditions is achieved, which reduces the amount of catalyst, increases the yield of primary amines, and enhances the stability and safety of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080623A_ABST
    Figure CN119080623A_ABST
Patent Text Reader

Abstract

The invention discloses application of a catalyst to preparation of primary amine by catalyzing nitrile compound hydrogenation, and relates to the technical field of catalysts. The catalyst comprises a nickel-based catalyst and a metal oxide; wherein the metal oxide comprises any one or a combination of at least two of tungsten oxide, molybdenum oxide or vanadium oxide. The catalyst provided by the invention can catalyze hydrogenation reaction of nitrile compounds to realize synthesis of high-selectivity primary amine, the catalytic reaction condition is mild, the substrate conversion rate is high, and meanwhile, the catalyst has the characteristics of high activity, high stability and reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to application of a catalyst in catalyzing the hydrogenation of nitrile compounds to prepare primary amines. Background Art

[0002] Primary amines and their derivatives play a very important role in medicine, dyes and pesticides, and the selective hydrogenation of nitrile compounds is an effective method for preparing primary amine molecules. In the hydrogenation of nitrile compounds, in addition to the target product primary amine, many by-products such as imine dimers and trimers are also produced, resulting in low selectivity of the catalyst for primary amines.

[0003] In order to develop a highly selective nitrile hydrogenation catalyst, Lu et al. deposited a layer of Pd atoms on the Ni surface by atomic deposition technology in 2019. Although the cyanide hydrogenation performance of the Ni-based catalyst was greatly improved, the secondary amine product was mainly obtained (Nat. Commun., 2019, 10, 4998). In 2018, Beller and V. Jagadeesh et al. developed a Co@Co3O4 / C supported catalyst with a graphite carbon layer on the surface by pyrolyzing carbon-supported Co-TPA-MOF precursor. Under the conditions of 120°C, 2.5MPa H2, and 0.5MPa NH3, a 97% primary amine yield can be achieved after 15h of reaction (Chem. Sci., 2018, 9, 8553). In 2021, Beller et al. prepared Fe / Fe-O@SiO2 catalyst by pyrolysis of Fe(OAc)2-loaded SiO2. The interior of the catalyst is α-Fe nanoparticles, the interface is fayalite (FeSi2O4) with a clear structure, and the surface of SiO2 is covered with a layer of amorphous Fe(III) oxide (Nat. Catal., 2022, 5, 20); Beller et al. found that modifying Al film or Al(iPrO)3 ​​in the Fe / Fe-O@SiO2 catalytic system can greatly improve the catalyst activity. Primary amines were prepared with a yield of 96% after reacting for 24 hours at 120°C, 5MPa H2, and 0.5-0.7MPa NH3.

[0004] Although the above methods achieve good primary amine yields from different angles and methods, the reaction conditions of the catalytic system are harsh (such as 120°C, 5MPa H2, 0.5-0.7MPa NH3), and the amount of catalyst required is large (such as 8.5mol% Fe); in addition, the use of pure ammonia limits its industrial application to a certain extent.

[0005] Therefore, achieving highly active and highly selective hydrogenation of nitrile compounds under mild conditions through surface and interface modification is a technical problem that needs to be solved urgently, and it has broad application prospects for industrial catalysts for cyanide hydrogenation.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The purpose of the present invention is to provide a catalyst for the hydrogenation of nitrile compounds to prepare primary amines. The purpose of the present invention is to modify nickel nanoparticles by tungsten oxide, molybdenum oxide or vanadium oxide so that the catalyst can catalyze the hydrogenation of nitrile compounds to produce primary amine compounds with high selectivity and conversion rate.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a use of a catalyst in catalyzing the hydrogenation of nitrile compounds to prepare primary amines, wherein the catalyst comprises a nickel-based catalyst and a metal oxide;

[0010] The metal oxide includes any one of tungsten oxide, molybdenum oxide or vanadium oxide, or a combination of at least two of them.

[0011] Furthermore, the metal oxide forms a coating layer on the surface of the nickel-based catalyst.

[0012] Furthermore, the 4f orbital binding energy of the tungsten element in the tungsten oxide is between 30 and 42 eV.

[0013] Furthermore, the 3d orbital binding energy of the molybdenum element in the molybdenum oxide is between 228 and 239 eV.

[0014] Furthermore, the 2p orbital binding energy of the vanadium element in the vanadium oxide is between 510 and 530 eV.

[0015] Preferably, the loading amount of the metal oxide accounts for 0.01 to 50 wt % of the total mass of the catalyst.

[0016] Furthermore, the nickel-based catalyst is selected from any one of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals, or a combination of at least two thereof.

[0017] Preferably, the supported nickel-based catalyst comprises a carrier and nickel nanoparticles supported on the carrier.

[0018] Preferably, the loading amount of the nickel nanoparticles accounts for 1 to 60 wt % of the total mass of the supported nickel-based catalyst.

[0019] Preferably, the carrier is selected from any one or a combination of at least two of a carbon carrier, Al2O3, SiO2, MgO, TiO2, ZrO2 or CeO2.

[0020] Preferably, the carbon carrier is selected from any one of activated carbon, carbon nanotubes, carbon black or mesoporous carbon, or a combination of at least two thereof.

[0021] In a second aspect, the present invention provides a method for preparing the catalyst as described in the first aspect, the method for preparing the catalyst comprising the following steps:

[0022] The nickel-based catalyst and a metal precursor are mixed, calcined and reduced to obtain the catalyst; wherein the metal precursor includes any one of a tungsten precursor, a molybdenum precursor or a vanadium precursor, or a combination of at least two thereof.

[0023] Furthermore, the nickel-based catalyst is selected from any one of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals, or a combination of at least two thereof.

[0024] Furthermore, the tungsten precursor is selected from any one of ammonium metatungstate, ammonium paratungstate, sodium tungstate or ammonium tungstate, or a combination of at least two thereof.

[0025] Furthermore, the molybdenum precursor is selected from ammonium tetramolybdate and / or ammonium heptamolybdate.

[0026] Furthermore, the vanadium precursor is selected from any one of sodium metavanadate, sodium pyrovanadate, ammonium metavanadate or sodium orthovanadate, or a combination of at least two thereof.

[0027] Furthermore, the mass ratio of the metal precursor to the nickel-based catalyst is (0.01-1):1.

[0028] Preferably, the calcination is carried out under a protective gas atmosphere; wherein the protective gas is selected from any one of nitrogen, argon or hydrogen, or a combination of at least two of them.

[0029] Preferably, the calcination temperature is 100-600° C., and the calcination time is 1-12 hours.

[0030] Preferably, the reduction is carried out under a reducing gas atmosphere; wherein the reducing gas is selected from hydrogen or a hydrogen-argon mixture.

[0031] Preferably, the volume percentage of hydrogen in the hydrogen-argon mixed gas is 1-50 vol%.

[0032] Preferably, the reduction temperature is 100-500° C., and the reduction time is 1-4 hours.

[0033] Furthermore, the supported nickel-based catalyst is prepared by the following steps: adsorbing a nickel salt precursor onto a carrier, followed by calcination and reduction to obtain the supported nickel-based catalyst.

[0034] Preferably, the supported nickel-based catalyst is prepared by the following steps:

[0035] (a) dispersing the support in a solvent, mixing with a solution containing a nickel precursor, stirring and drying to obtain a solid phase;

[0036] (b) calcining and reducing the solid phase to obtain the supported nickel-based catalyst.

[0037] Preferably, in step (a), the nickel precursor is selected from any one or a combination of at least two of Ni(acac)2, Ni(CH3COO)2, Ni(NO3)2, Ni2SO4 or NiCl2.

[0038] Preferably, in step (a), the mass ratio of the nickel precursor to the nanoparticle carrier is (0.01-1.5):1.

[0039] Preferably, in step (b), the calcination reduction is carried out in a hydrogen-argon mixed gas atmosphere.

[0040] Preferably, the volume percentage of hydrogen in the hydrogen-argon mixed gas is 1-50 vol%.

[0041] Preferably, in step (b), the temperature of the calcination reduction is 100 to 600° C., and the time of the calcination reduction is 1 to 12 hours.

[0042] In a third aspect, the present invention provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds, the method comprising the following steps:

[0043] The catalyst, nitrile compound, base and reaction solvent are mixed and contacted with hydrogen to carry out catalytic reaction to obtain primary amine compounds;

[0044] Wherein, the catalyst includes the catalyst or a catalyst obtained by the method for preparing the catalyst.

[0045] Furthermore, the structural formula of the nitrile compound is shown in Formula I below:

[0046]

[0047]

[0048] Wherein, R2 and R3 represent any organic functional group substituents at different positions of the benzene ring.

[0049] Preferably, the substituent is selected from any one of H, halogen, C1-C6 straight chain or branched alkyl, C1-C6 straight chain or branched alkoxy, or a combination of at least two of them.

[0050] Preferably, the nitrile compound is selected from any one of benzonitrile, 2,4-dimethylbenzonitrile, p-chlorobenzonitrile, p-fluorobenzonitrile, o-chlorobenzonitrile, p-bromobenzonitrile, p-methylbenzonitrile, m-methylbenzonitrile, o-methylbenzonitrile, p-methoxybenzonitrile, o-methoxybenzonitrile, p-ethylbenzonitrile or p-tert-butylbenzonitrile.

[0051] Preferably, the base comprises NH3, preferably aqueous ammonia and / or methanolic ammonia solution.

[0052] Preferably, the reaction solvent is selected from any one or a combination of at least two of water, methanol, ethanol, acetonitrile, toluene, tetrahydrofuran, γ-butyrolactone, chlorobenzene, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl carbonate, dioxane, n-hexane or cyclohexane.

[0053] Preferably, the temperature of the catalytic reaction is 40 to 90° C., and the time of the catalytic reaction is 2 to 72 hours.

[0054] Preferably, the pressure of the hydrogen is 0.5-3 MPa.

[0055] Preferably, the molar ratio of the nickel element to the nitrile compound in the catalyst is 1:(20-400).

[0056] Compared with the prior art, the present invention has the following beneficial effects:

[0057] (1) Ni@WO of the present invention x / Carrier, Ni@MoO x / carrier or Ni@VO x / Carrier-supported catalysts can catalyze the hydrogenation reaction of nitrile compounds under mild conditions, with low catalyst dosage, high activation activity and high selectivity.

[0058] (2) The modification strategy of tungsten oxide, molybdenum oxide or vanadium oxide described in the present invention is universal and can be applied to, but not limited to, the modification of nickel-based catalysts such as nickel-based supported catalysts, Raney nickel catalysts, and nickel nanocrystalline catalysts, thereby greatly improving the hydrogenation performance of nitrile compounds of nickel-based catalysts.

[0059] (3) The catalyst of the present invention has high selectivity and only requires a small amount of aqueous ammonia as a base to achieve a high primary amine yield, which effectively reduces the corrosion of the base to the equipment and improves the safety and feasibility of the equipment process.

[0060] (4) The catalyst of the present invention has high stability and can be reused many times without observing a decrease in catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0062] Figure 1 The Ni / C and Ni@WO prepared in Example 1 x Powder X-ray diffraction spectrum of the catalyst.

[0063] Figure 2 Ni@WO prepared in Example 1 x XPS characterization of the Mg / C catalyst.

[0064] Figure 3 The catalyst Ni@WO prepared in Example 1 x Transmission electron micrograph of / C.

[0065] Figure 4 The catalyst Ni@WO prepared in Example 1 x / C is a cyclic stability test diagram for hydrogenation of nitrile compounds.

[0066] Figure 5 Ni / C and Ni@WO prepared in Example 1 x / C catalytic 2,4-dimethylbenzonitrile hydrogenation performance diagram. DETAILED DESCRIPTION

[0067] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0068] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0069] In this specification, the term "Ni / C" means that nickel nanoparticles are supported on a carbon support.

[0070] In this specification, the term "Ni@WO x / C" means that the nickel nanoparticles are loaded on the carbon support and modified by calcination reduction of tungsten oxide.

[0071] In this specification, the term "Ni@MoO x / C" means that the nickel nanoparticles are loaded on the carbon support and modified by calcination reduction of molybdenum oxide.

[0072] In this specification, the term "Ni@VO x / C" means that the nickel nanoparticles are supported on a carbon support and modified by calcination reduction of vanadium oxide.

[0073] In this specification, the term "Raney Ni" means a Raney nickel catalyst.

[0074] In this specification, the term "Raney Ni@WO x ” indicates a Raney nickel catalyst which is modified by calcination reduction of tungsten oxide.

[0075] In this specification, the term "Ni" means nickel nanocrystals.

[0076] In this specification, the term "Ni@WO x "NP" means nickel nanocrystals, which are modified by calcination reduction of tungsten oxide.

[0077] In this specification, the term "substituted" refers to the replacement of a hydrogen atom in a compound by another substituent. The position is not limited to a specific position, as long as the hydrogen at the position can be replaced by a substituent. When two or more substituents are present, the two or more substituents may be the same or different.

[0078] In the present specification, the term "halogen" includes fluorine (F), chlorine (Cl), bromine (Br) and iodine (I).

[0079] In this specification, the term "alkyl" refers to a monovalent substituent derived from a straight or branched saturated hydrocarbon having a certain number of carbon atoms. Specifically, "C1-C6 straight or branched alkyl" represents a monovalent substituent of a straight or branched saturated hydrocarbon having 1 to 6 carbon atoms, and examples thereof include but are not limited to methyl, ethyl, propyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl or n-hexyl, etc.

[0080] In this specification, the term "alkoxy" is composed of an alkyl-oxy group (RO-), wherein the oxygen atom is connected to the carbon atom of the alkyl group by a single bond. Specifically, "C1-C6 straight or branched alkoxy" represents a straight or branched alkoxy group having 1 to 6 carbon atoms, examples of which include but are not limited to methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or 2-methoxyethoxy, etc.

[0081] In this specification, the term "aryl" is an aromatic group. It is a general term for a monovalent group left after removing a hydrogen atom from the aromatic carbon of an aromatic hydrocarbon molecule. It is usually represented by Ar. Specifically, "C6-C16 aromatic group" represents an aromatic group with 6 to 16 carbon atoms, such as phenyl, o-tolyl, naphthyl, anthracenyl, pyrenyl, etc.

[0082] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0083] In a first aspect, the present invention provides a catalyst comprising a nickel-based catalyst and a metal oxide; wherein the metal oxide comprises any one of tungsten oxide, molybdenum oxide or vanadium oxide, or a combination of at least two thereof.

[0084] In the present invention, the nickel-based catalyst is modified by the above-mentioned specific metal oxide (any one of tungsten oxide, molybdenum oxide or vanadium oxide or a combination of at least two thereof), and the modified metal oxide (any one of tungsten oxide, molybdenum oxide or vanadium oxide or a combination of at least two thereof) forms a coating layer on the surface of the nickel-based catalyst, providing a large number of B acid sites, promoting hydrogen transfer during the hydrogenation of nitrile compounds, so that the prepared catalyst can catalyze the hydrogenation of nitrile compounds with high activity and high selectivity to prepare primary amine products. At the same time, the presence of a large number of B acid sites makes the product primary amine protonated and easy to desorb, avoiding the catalyst from being poisoned by the primary amine ligand, and ensuring the catalyst cycle stability.

[0085] In an optional embodiment, the catalyst includes a nickel-based catalyst and a metal oxide active component coated on the surface of the nickel-based catalyst.

[0086] In an optional embodiment, the metal oxide forms a coating layer on the surface of the nickel-based catalyst.

[0087] It should be noted that, in the present invention, the coating layer formed by the metal oxide can completely wrap the nickel nanoparticles; and / or, the coating layer formed by the metal oxide partially wraps the nickel nanoparticles and is partially loaded on the nanoparticle carrier; and / or, the metal oxide and the surface of the nickel nanoparticles form a specific metal-metal oxide active interface, including any one of metal-metal tungsten oxide, metal-metal tungsten oxide or metal-metal vanadium oxide active interfaces or a combination of at least two of them.

[0088] In an optional embodiment, the 4f orbital binding energy of the tungsten element in the tungsten oxide is 30-42eV, for example, it can be 30eV, 31eV, 32eV, 33eV, 34eV, 35eV, 36eV, 37eV, 38eV, 39eV, 40eV, 41eV, 42eV, etc.

[0089] In an optional embodiment, the 3d orbital binding energy of the molybdenum element in the molybdenum oxide is between 228 and 239 eV, for example, 228 eV, 229 eV, 230 eV, 231 eV, 232 eV, 233 eV, 234 eV, 235 eV, 236 eV, 237 eV, 238 eV, 239 eV, etc.

[0090] In an optional embodiment, the 2p orbital binding energy of the vanadium element in the vanadium oxide is 510-530eV, for example, it can be 510eV, 512eV, 514eV, 516eV, 518eV, 520eV, 522eV, 524eV, 526eV, 528eV, 530eV, etc.

[0091] In an optional embodiment, the chemical formula of the metal oxide is MO x ;

[0092] Wherein, M represents a metal element, such as tungsten (W), molybdenum (Mo), and vanadium (V); wherein 1≤x≤4; and x can be, for example, 1, 2, 3, 4, etc.

[0093] More specifically, the chemical formula of the tungsten oxide is WO x ; Wherein, 1≤x≤4; x can be, for example, 1, 2, 3, 4, etc.

[0094] More specifically, the chemical formula of the molybdenum oxide is MoO x ; Wherein, 1≤x≤4; x can be, for example, 1, 2, 3, 4, etc.

[0095] More specifically, the chemical formula of the vanadium oxide is VO x ; Wherein, 1≤x≤4; x can be, for example, 1, 2, 3, 4, etc.

[0096] In an optional embodiment, the loading of the metal oxide is 0.01 to 50 wt% of the total mass of the catalyst, for example, 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.5 wt%, 0.6 wt%, 0.8 wt%, 1 wt%, 1.5 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt%, 20 wt%, 22 wt%, 25 wt%, 28 wt%, 30 wt%, 32 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt% and the like.

[0097] In an optional embodiment, the nickel-based catalyst is selected from any one or a combination of at least two of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals.

[0098] In an optional embodiment, the supported nickel-based catalyst includes a carrier and nickel nanoparticles supported on the carrier.

[0099] In an optional embodiment, the loading of the nickel nanoparticles is 1 to 60 wt% of the total mass of the supported nickel-based catalyst, for example, it can be 1 wt%, 1.5 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt%, 20 wt%, 22 wt%, 25 wt%, 28 wt%, 30 wt%, 32 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt% and the like.

[0100] It should be noted that, in the present invention, the catalytic performance of the catalyst for selectively catalyzing the hydrogenation reduction of nitrile compounds to primary amines can be further improved by controlling the loading of metal oxides and / or the loading of nickel nanoparticles.

[0101] In an optional embodiment, the carrier is selected from any one or a combination of at least two of a carbon carrier, Al2O3, SiO2, MgO, TiO2, ZrO2 or CeO2;

[0102] In an optional embodiment, the carbon carrier is selected from any one of activated carbon, carbon nanotubes, carbon black or mesoporous carbon, or a combination of at least two thereof.

[0103] In a second aspect, the present invention provides a method for preparing the catalyst as described in the first aspect, the method for preparing the catalyst comprising the following steps:

[0104] The nickel-based catalyst and a metal precursor are mixed, calcined and reduced to obtain the catalyst; wherein the metal precursor includes any one of a tungsten precursor, a molybdenum precursor or a vanadium precursor, or a combination of at least two thereof.

[0105] In the present invention, nickel nanoparticles are first loaded on the carrier by a high-temperature reduction method to prepare a loaded nickel-based catalyst; then the Ni / carrier is mixed with a tungsten precursor, a molybdenum precursor or a vanadium precursor and then calcined and reduced to obtain the catalyst. The method of the present invention can well form a coating layer of tungsten oxide, molybdenum oxide or vanadium oxide on the surface of the nickel nanoparticles, reflecting a strong metal-metal oxide interaction, effectively avoiding the aggregation of nickel nanoparticles during the hydrogenation reaction, and ensuring the stability of the catalyst. At the same time, the coating layer of tungsten oxide, molybdenum oxide or vanadium oxide provides a large number of B acid sites, which is beneficial to the activation of nitrile compounds and hydrogen transfer during the hydrogenation process, thereby greatly improving the hydrogenation performance of the nickel-based catalyst.

[0106] In an optional embodiment, the tungsten precursor is selected from any one of ammonium metatungstate, ammonium paratungstate, sodium tungstate or ammonium tungstate, or a combination of at least two thereof.

[0107] In an alternative embodiment, the molybdenum precursor is selected from ammonium tetramolybdate and / or ammonium heptamolybdate.

[0108] In an optional embodiment, the vanadium precursor is selected from any one of sodium metavanadate, sodium pyrovanadate, ammonium metavanadate or sodium orthovanadate, or a combination of at least two thereof.

[0109] It should be noted that in the preparation method of the catalyst of the present invention, by selecting the above-mentioned specific tungsten precursor, molybdenum precursor or vanadium precursor, the method of the present invention can well form a coating layer of tungsten oxide, molybdenum oxide or vanadium oxide on the surface of nickel nanoparticles, reflecting the strong interaction between metal and metal oxide, effectively avoiding the aggregation of nickel nanoparticles during the hydrogenation reaction, and ensuring the stability of the catalyst. At the same time, the coating layer of tungsten oxide, molybdenum oxide or vanadium oxide provides a large number of B acid sites, which is conducive to the activation of nitrile compounds and hydrogen transfer during the hydrogenation process, thereby greatly improving the hydrogenation performance of nickel-based catalysts.

[0110] In an optional embodiment, the nickel-based catalyst is selected from any one or a combination of at least two of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals.

[0111] In an optional embodiment, the mass ratio of the metal precursor to the nickel-based catalyst is (0.01-1):1, for example, it can be 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.15:1, 0.2:1, 025:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, etc.

[0112] It should be noted that, in the present invention, the loading amount of the metal oxide can be controlled by adjusting the mass ratio of the nickel-based catalyst to the metal precursor.

[0113] In an optional embodiment, the calcination is performed under a protective gas atmosphere.

[0114] In an optional embodiment, the protective gas is selected from any one of nitrogen, argon or hydrogen, or a combination of at least two of them.

[0115] In an optional embodiment, the calcination temperature is 100-600°C, for example, it can be 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, etc.

[0116] In an optional embodiment, the calcination time is 1 to 12 h, for example, it can be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h, 8 h, 8.5 h, 9 h, 9.5 h, 10 h, 10.5 h, 11 h, 1.5 h, 12 h, etc.

[0117] In an optional embodiment, the reduction is performed under a reducing gas atmosphere.

[0118] In an optional embodiment, the reducing gas is selected from hydrogen or a hydrogen-argon mixture.

[0119] In an optional embodiment, the volume percentage of hydrogen in the hydrogen-argon mixture is 1 to 50 vol%, for example, it can be 1 vol%, 2 vol%, 3 vol%, 4 vol%, 5 vol%, 6 vol%, 7 vol%, 8 vol%, 9 vol%, 10 vol%, 15 vol%, 20 vol%, 25 vol%, 30 vol%, 40 vol%, 45 vol%, 50 vol%, etc.

[0120] In an optional embodiment, the reduction temperature is 100-500°C, for example, it can be 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, etc.

[0121] In an optional embodiment, the reduction time is 1 to 4 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, etc.

[0122] In an optional embodiment, when the nickel-based catalyst is selected from a supported nickel-based catalyst, the method for preparing the catalyst comprises the following steps:

[0123] (1) adsorbing a metal nickel salt precursor onto the carrier, and preparing the supported nickel-based catalyst after calcination and reduction;

[0124] (2) The nickel-based catalyst and a metal precursor are mixed, and the mixture is calcined and reduced to obtain the catalyst; wherein the nickel-based catalyst comprises any one of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals; wherein the metal precursor comprises any one of a tungsten precursor, a molybdenum precursor or a vanadium precursor, or a combination of at least two thereof.

[0125] In an optional embodiment, the supported nickel-based catalyst is prepared by the following steps:

[0126] (a) dispersing the support in a solvent, mixing with a solution containing a nickel precursor, stirring and drying to obtain a solid phase;

[0127] (b) calcining and reducing the solid phase to obtain the supported nickel-based catalyst.

[0128] It should be noted that in the preparation process of the solid phase in the above step (a), the nanoparticle carrier is dispersed in the solvent, and then the solution containing the nickel precursor is added to complete the mixing. It is also necessary to stir again so that the nanoparticle carrier can fully absorb the nickel precursor, and then dry it.

[0129] In an optional embodiment, in step (a), the nickel precursor is selected from any one or a combination of at least two of Ni(acac)2, Ni(CH3COO)2, Ni(NO3)2, Ni2SO4 or NiCl2.

[0130] In an optional embodiment, in step (a), the mass ratio of the nickel precursor to the nanoparticle carrier is (0.01-1.5):1, for example, it can be 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.15:1, 0.2:1, 025:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, etc.

[0131] In an optional embodiment, in step (a), the stirring time is 1 to 10 hours, for example, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, etc.

[0132] In an optional embodiment, in step (a), the drying temperature is 20-120°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, etc.

[0133] In an optional embodiment, in step (a), the drying time is 1 to 48 hours, for example, 1 hour, 2 hours, 4 hours, 6 hours, 12 hours, 18 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, etc.

[0134] In an optional embodiment, in step (a), the solvent is water.

[0135] In an optional embodiment, in step (a), the mass ratio of the nanoparticle carrier to the solvent is 1:(1-50), for example, it can be 1:1, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, etc.

[0136] In an optional embodiment, in step (a), the solvent in the solution containing the nickel precursor is water.

[0137] In an optional embodiment, in step (a), in the solution containing nickel precursor, the mass ratio of the nickel precursor to the solvent is 1:(1-50), for example, it can be 1:1, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, etc.

[0138] In an optional embodiment, in step (b), the calcination reduction is carried out in a hydrogen-argon mixed gas atmosphere.

[0139] In an optional embodiment, in step (b), the volume percentage of hydrogen in the hydrogen-argon mixture is 1 to 50 vol%, for example, it can be 1 vol%, 2 vol%, 3 vol%, 4 vol%, 5 vol%, 6 vol%, 7 vol%, 8 vol%, 9 vol%, 10 vol%, 15 vol%, 20 vol%, 25 vol%, 30 vol%, 40 vol%, 45 vol%, 50 vol%, etc.

[0140] In an optional embodiment, in step (b), the calcination reduction temperature is 100-600°C, for example, it can be 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C, 360°C, 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, etc.

[0141] In an optional embodiment, in step (b), the calcination reduction time is 1 to 12 h, for example, it can be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h, 8 h, 8.5 h, 9 h, 9.5 h, 10 h, 10.5 h, 11 h, 1.5 h, 12 h, etc.

[0142] In a third aspect, the present invention provides a use of the catalyst as described in the first aspect, or the catalyst obtained by the preparation method of the catalyst as described in the second aspect, in catalyzing the hydrogenation of nitrile compounds to prepare primary amines.

[0143] In a fourth aspect, the present invention provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds, the method comprising the following steps:

[0144] The catalyst, nitrile compound, base and reaction solvent are mixed and contacted with hydrogen to carry out catalytic reaction to obtain primary amine compounds.

[0145] Wherein, the catalyst includes the catalyst as described in the first aspect, or the catalyst obtained by the preparation method of the catalyst as described in the second aspect.

[0146] In an optional embodiment, the structural formula of the nitrile compound is shown in Formula I below:

[0147]

[0148] Wherein, R2 and R3 represent any organic functional group substituents at different positions of the benzene ring.

[0149] In an optional embodiment, the substituent is selected from any one or a combination of at least two of H, halogen, straight-chain or branched alkyl, straight-chain or branched alkoxy, and aryl.

[0150] In an optional embodiment, the straight chain or branched chain alkyl group includes a C1-C6 straight chain or branched chain alkyl group.

[0151] In an optional embodiment, the straight chain or branched chain alkoxy group includes a C1 to C6 straight chain or branched chain alkoxy group.

[0152] In an optional embodiment, the aromatic group includes a C6-C16 aromatic group.

[0153] In an optional embodiment, the nitrile compound is selected from any one of benzonitrile, 2,4-dimethylbenzonitrile, p-chlorobenzonitrile, p-fluorobenzonitrile, o-chlorobenzonitrile, p-bromobenzonitrile, p-methylbenzonitrile, m-methylbenzonitrile, o-methylbenzonitrile, p-methoxybenzonitrile, o-methoxybenzonitrile, p-ethylbenzonitrile or p-tert-butylbenzonitrile.

[0154] In an optional embodiment, the base comprises NH3, preferably aqueous ammonia and / or methanolic ammonia solution.

[0155] In an optional embodiment, the reaction solvent is selected from any one of water, methanol, ethanol, acetonitrile, toluene, tetrahydrofuran, γ-butyrolactone, chlorobenzene, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl carbonate, dioxane, n-hexane or cyclohexane, or a combination of at least two thereof.

[0156] In an optional embodiment, the temperature of the catalytic reaction is 40-90°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, etc.

[0157] In an optional embodiment, the catalytic reaction time is 2 to 72 hours, for example, it can be 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 15h, 20h, 24h, 25h, 30h, 35h, 40h, 45h, 50h, 55h, 60h, 65h, 70h, 72h, etc.

[0158] In an optional embodiment, the pressure of the hydrogen is 0.5-3 MPa, for example, 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, etc.

[0159] In an optional embodiment, the molar ratio of the nickel element to the nitrile compound in the catalyst is 1:(20-400), for example, it can be 1:20, 1:40, 1:60, 1:80, 1:100, 1:120, 1:140, 1:160, 1:180, 1:200, 1:220, 1:240, 1:260, 1:280, 1:300, 1:320, 1:340, 1:360, 1:380, 1:400, etc.

[0160] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0161] Example 1

[0162] This embodiment provides a catalyst, which is prepared by the following steps:

[0163] S1. Preparation of nickel carrier:

[0164] 1.6 g of activated carbon (carrier) was dispersed in 200 mL of water in a 500 mL beaker, and then 40 mL of an aqueous solution containing 2.0 g of Ni(NO3)2·6H2O (precursor, Ni is an active metal) was added under stirring, and stirring was continued for 4 h; then it was placed in an oven at 100 ° C. and dried for 24 h to obtain a solid phase; the solid phase was placed in a porcelain boat, placed in a tubular furnace, the heating rate was set to 3 ° C / min, the temperature was raised to 450 ° C, and calcined for 2 h in an atmosphere of a hydrogen-argon mixture of 5 vol% hydrogen, then naturally cooled to room temperature, and the gas was turned off to obtain a Ni / C solid powder with a Ni metal loading of 20 wt%.

[0165] S2. Metal oxide coating:

[0166] 100 mg of ammonium metatungstate was taken, mixed with 2 g of Ni / C solid powder, and then put into a porcelain boat, loaded into a tube furnace, introduced into a N2 atmosphere, set the heating rate to 2 ° C / min, heated to 300 ° C for 2 h, and then naturally cooled to room temperature; then the gas was replaced with a hydrogen-argon mixture with 5 vol% hydrogen, the heating rate was set to 4 ° C / min, the temperature was raised to 150 ° C, and the reduction reaction was carried out for 1 h, and then naturally cooled to room temperature, and the gas was turned off to obtain Ni@WO with a Ni metal loading of 20wt%. x / CW-5% catalyst.

[0167] The catalyst prepared above was characterized:

[0168] Figure 1 The Ni / C and Ni@WO prepared in Example 1 x The powder X-ray diffraction spectrum of the / CW-5% catalyst shows that there is no significant change in the XRD diffraction peak before and after the tungsten oxide modification, indicating that the nickel nanoparticle lattice has not changed after the modification, and the tungsten oxide is mainly deposited on the surface of the nickel nanoparticles. At the same time, XPS characterization shows that there is an obvious W element signal on the surface of the nickel nanoparticles ( Figure 2 ), further supporting the conclusion that tungsten oxide is mainly deposited on the surface of nickel nanoparticles. Figure 3 It's Ni@WO x The transmission electron microscopy image of the / CW-5% catalyst shows that the Ni NPs are uniformly dispersed on the surface of the activated carbon support with uniform size. At the same time, no tungsten oxide nanoparticles were observed, indicating that tungsten oxide is uniformly deposited on the surface of the nickel nanoparticles in a molecular layer deposition manner.

[0169] Example 2

[0170] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 2.0 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / CW-0.1% catalyst.

[0171] Example 3

[0172] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 10 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / CW-0.5% catalyst.

[0173] Example 4

[0174] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 20 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20 wt% Ni@WO is prepared. x / CW-1% catalyst.

[0175] Example 5

[0176] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 50 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / CW-2.5% catalyst.

[0177] Example 6

[0178] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 200 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20 wt% Ni@WO is prepared. x / CW-10% catalyst.

[0179] Example 7

[0180] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 400 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20 wt% Ni@WO is prepared. x / CW-20% catalyst.

[0181] Example 8

[0182] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 800 mg, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / CW-40% catalyst.

[0183] Example 9

[0184] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the amount of ammonium metatungstate used is 2g, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / CW-100% catalyst.

[0185] Test Example 1

[0186] Study on the Effect of Tungstate Dosage on Catalytic Activity

[0187] Test sample: catalyst provided in Examples 1 to 9;

[0188] Test method: 16 mg of each of the above samples were dissolved in 5 mL of methanol solution with 5 mmol of benzonitrile and 500 μL of ammonia water, and added to a high-pressure reactor. 2.5 MPa of hydrogen was introduced, the temperature was raised to 80°C, the speed was set to 800 rpm, and after reacting for 3 hours, 50 μL of the reaction solution was taken and the yield of benzylamine was detected by gas chromatography.

[0189] The test results are shown in Table 1 below:

[0190] Table 1

[0191]

[0192]

[0193] As can be seen from Table 1, with the increase in the amount of tungstate used, the activity of the modified catalyst increases significantly; when the amount of tungstate increases to more than 2.5%, the yield of benzonitrile reaches more than 95%; further, when the amount of tungstate is higher than 40%, the yield of benzonitrile begins to decrease. This is because the use of excessive tungstate results in the generation of a large amount of tungsten oxides to wrap the nickel on the surface, and the hydrogen dissociation is subject to certain restrictions, so the reaction activity decreases. Therefore, the method of tungstate modified nickel-based catalyst provided by the present invention can effectively improve the catalytic efficiency of the catalyst benzonitrile hydrogenation reaction.

[0194] Furthermore, 16 mg of Ni@WO prepared in Example 1 was added x The / C catalyst was cycled 5 times according to the above selective catalytic method for benzonitrile, each reaction was 3 hours, and the conversion rate and selectivity of benzylamine were tested for each reaction. The results are as follows Figure 4As shown in Figure 2, the catalyst showed no obvious deactivation during the 5-cycle test, further confirming its high stability. Figure 4 It is shown that the catalyst provided by the present invention can maintain a cyclic test of 3 hours per reaction for at least 5 times, and has significant stability. This is because the surface tungsten oxide coating layer effectively inhibits the agglomeration of nickel nanoparticles during the hydrogenation process, greatly improves the catalyst stability, reduces the reaction cost and promotes the industrialization of the product. The catalyst of the present invention can selectively catalyze the hydrogenation of benzonitrile to benzylamine, and the yield of benzylamine is 95%, and has excellent catalytic activity.

[0195] Example 10

[0196] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the tungsten precursor is replaced with ammonium tungstate of equal mass, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / C-AT catalyst.

[0197] Embodiment 11

[0198] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the tungsten precursor is replaced with ammonium paratungstate of equal mass, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / C-APT catalyst.

[0199] Example 12

[0200] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the tungsten precursor is replaced with an equal mass of sodium tungstate, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / C-ST catalyst.

[0201] Embodiment 13

[0202] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the tungsten precursor is replaced with an equal mass of ammonium tetramolybdate, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / C-ATM catalyst.

[0203] Embodiment 14

[0204] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the tungsten precursor is replaced with an equal mass of ammonium heptamolybdate, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / C-AHM catalyst.

[0205] Embodiment 15

[0206] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the tungsten precursor is replaced with an equal mass of ammonium metavanadate, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / C-AMV catalyst.

[0207] Test Example 2

[0208] Investigation of the effect of metal precursors on the catalytic activity of catalysts

[0209] Test samples: the catalyst provided in Example 1, and the catalysts provided in Examples 10 to 15;

[0210] Test method: Same as test example 1.

[0211] The test results are shown in Table 2 below:

[0212] Table 2

[0213]

[0214]

[0215] As can be seen from Table 2, the use of different tungstates, molybdates, and vanadates to modify the Ni / C catalyst has achieved good results. The activity of the modified catalyst is significantly increased, and the yield of benzonitrile is more than 93%. Therefore, the method of modifying the nickel-based catalyst with tungstates, molybdates, and vanadates provided by the present invention can effectively improve the catalytic efficiency of the catalyst benzonitrile hydrogenation reaction.

[0216] Example 16

[0217] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the activated carbon is replaced by an equal mass of aluminum oxide as a nanoparticle carrier, the reducing atmosphere is hydrogen, the reducing temperature is 450°C, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / Al2O3 catalyst.

[0218] Embodiment 17

[0219] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the activated carbon is replaced by an equal mass of silicon dioxide, the reducing atmosphere is hydrogen, the reducing temperature is 450°C, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / SiO2 catalyst.

[0220] Embodiment 18

[0221] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the activated carbon is replaced with an equal mass of titanium dioxide, the reducing atmosphere is hydrogen, the reducing temperature is 450°C, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / TiO2 catalyst.

[0222] Embodiment 19

[0223] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the activated carbon is replaced with an equal mass of magnesium oxide, the reducing atmosphere is hydrogen, the reducing temperature is 550°C, and the remaining preparation steps and material selection are the same as the embodiment 1, to prepare 20wt% Ni@WO x / MgO catalyst.

[0224] Embodiment 20

[0225] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the Ni / C catalyst is replaced by an equal mass of Raney nickel catalyst, and the remaining preparation steps and material selection are the same as those in the embodiment 1 to prepare Raney Ni@WO x catalyst.

[0226] Embodiment 21

[0227] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the Ni / C catalyst is replaced by a nickel nanocrystalline catalyst of equal mass, and the remaining preparation steps and material selection are the same as the embodiment 1 to prepare Ni@WO x NP catalyst.

[0228] Test Example 3

[0229] Investigation on the catalytic activity of different nickel-based catalysts after modification

[0230] Test samples: the catalyst provided in Example 1, and the catalysts provided in Examples 16 to 21;

[0231] Test method: Same as test example 1.

[0232] The test results are shown in Table 3 below:

[0233] Table 3

[0234]

[0235] As can be seen from Table 3, using different tungstates to modify Ni / carrier-supported catalysts supported on different oxide carriers, Raney nickel catalysts, and nickel nanocrystalline catalysts all achieved good results. The activity of the modified catalysts increased significantly, and the yield of benzylamine reached more than 95%. Therefore, the method for modifying the nickel-based catalyst provided by the present invention can be applied to the modification of various nickel-based catalysts, and effectively improve the catalytic efficiency of the hydrogenation reaction of benzonitrile by the nickel-based catalyst.

[0236] Embodiment 22

[0237] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination temperature of this embodiment is 100°C, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-100 catalyst.

[0238] Embodiment 23

[0239] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination temperature of this embodiment is 150°C, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-150 catalyst.

[0240] Embodiment 24

[0241] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination temperature of this embodiment is 200°C, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-200 catalyst.

[0242] Embodiment 25

[0243] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination temperature of this embodiment is 250°C, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-250 catalyst.

[0244] Embodiment 26

[0245] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination temperature of this embodiment is 400°C, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-400 catalyst.

[0246] Test Example 4

[0247] Study on the Effect of Modification Temperature on Catalytic Activity of Catalyst

[0248] Test samples: the catalyst provided in Example 1, and the catalysts provided in Examples 22 to 26;

[0249] Test method: Same as test example 1.

[0250] The test results are shown in Table 4 below:

[0251] Table 4

[0252]

[0253]

[0254] As can be seen from Table 4, when the calcination temperature of the modified tungstate is increased from 100°C to 400°C, the activity of the modified nickel-based catalyst in catalyzing the hydrogenation of benzonitrile is significantly improved; in particular, when the modification temperature is 150-300°C, the yield of benzylamine reaches about 95%.

[0255] Embodiment 27

[0256] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination time of this embodiment is 0.5h, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-0.5h catalyst.

[0257] Embodiment 28

[0258] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination time of this embodiment is 1 hour, and the other preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / C-1h catalyst.

[0259] Embodiment 29

[0260] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination time of this embodiment is 4 hours, and the remaining preparation steps and material selection are the same as the embodiment 1, and 20wt% Ni@WO is prepared. x / C-4h catalyst.

[0261] Embodiment 30

[0262] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination time of this embodiment is 8 hours, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-8h catalyst.

[0263] Embodiment 31

[0264] This embodiment provides a catalyst, which is different from the embodiment 1 only in that the calcination time of this embodiment is 12 hours, and the remaining preparation steps and material selection are the same as those of the embodiment 1, and 20wt% Ni@WO is prepared. x / C-12h catalyst.

[0265] Test Example 5

[0266] Investigation on the effect of different modification time on the catalytic activity of catalyst

[0267] Test samples: the catalyst provided in Example 1, and the catalysts provided in Examples 27 to 31;

[0268] Test method: Same as test example 1.

[0269] The test results are shown in Table 5 below:

[0270] Table 5

[0271] sample Roasting time Benzylamine yield (%) Embodiment 27 0.5h 96.4 Embodiment 28 1h 96.0 Example 1 2h 95.6 Embodiment 29 4h 95.2 Embodiment 30 8h 92.5 Embodiment 31 12h 90.3

[0272] As can be seen from Table 5, the calcination time of tungstate modification is increased from 0.5h to 12h, and the activity of the modified nickel-based catalyst in catalyzing the hydrogenation of benzonitrile is significantly improved; in particular, the yield of benzylamine reaches about 95% when the calcination time is within 0.5-4h; and when the calcination time is further extended to 8h and 12h, the yield of benzonitrile is significantly reduced. This is because the long-term calcination makes the oxide layer on the surface of the nickel nanoparticles more dense, which is not conducive to the hydrogenation of hydrogen and benzonitrile substrate at the catalyst surface interface, so the activity is slightly reduced.

[0273] Comparative Example 1

[0274] In this comparative example, a 20 wt% carbon-supported nickel catalyst was prepared under the same preparation conditions as in Example 1, except that no modification of vanadate, tungstate or molybdate was performed, and the catalytic conditions were the same as in Example 1.

[0275] Comparative Example 2

[0276] This comparative example adopts the same preparation conditions as Example 16 to prepare a 20 wt% mass fraction of alumina-supported nickel catalyst, the difference being that no vanadate, tungstate or molybdate modification is performed, and the catalytic conditions are the same as Example 1.

[0277] Comparative Example 3

[0278] This comparative example adopts the same preparation conditions as Example 17 to prepare a 20 wt% mass fraction of silicon oxide supported nickel catalyst, the difference being that no vanadate, tungstate or molybdate modification is performed, and the catalytic conditions are the same as Example 1.

[0279] Comparative Example 4

[0280] This comparative example adopts the same preparation conditions as Example 18 to prepare a 20 wt% mass fraction of titanium dioxide supported nickel catalyst, the difference being that no vanadate, tungstate or molybdate modification is performed, and the catalytic conditions are the same as Example 1.

[0281] Comparative Example 5

[0282] This comparative example uses the same preparation conditions as Example 19 to prepare a 20 wt% mass fraction of magnesium oxide supported nickel catalyst, the difference being that no vanadate, tungstate or molybdate modification is performed, and the catalytic conditions are the same as Example 1.

[0283] Comparative Example 6

[0284] This comparative example uses the same Raney nickel catalyst as Example 20, except that no vanadate, tungstate or molybdate modification is performed, and the catalytic conditions are the same as Example 20.

[0285] Comparative Example 7

[0286] This comparative example uses the same nickel nanocatalyst as Example 21, except that no vanadate, tungstate or molybdate modification is performed, and the catalytic conditions are the same as Example 21.

[0287] Test Example 6

[0288] Investigation of the catalytic activity of catalysts modified by different metal precursors

[0289] Test sample: the catalyst provided in Comparative Examples 1 to 7;

[0290] Test method: Same as test example 1.

[0291] The test results are shown in Table 6 below:

[0292] Table 6

[0293] sample catalyst Benzylamine yield (%) Comparative Example 1 Ni / C 51.3 Comparative Example 2 <![CDATA[Ni / Al2O3]]> 63.6 Comparative Example 3 <![CDATA[Ni / SiO2]]> 66.8 Comparative Example 4 <![CDATA[Ni / TiO2]]> 49.1 Comparative Example 5 Ni / MgO 71.3 Comparative Example 6 Raney Ni 69.4 Comparative Example 7 Ni NP 58.2

[0294] As can be seen from Table 6, the Ni / carrier-supported catalysts supported on different oxide carriers without any vanadate, tungstate or molybdate modification, as well as the Raney nickel catalyst and the nickel nanocrystalline catalyst showed poor benzonitrile hydrogenation activity, and the yield of benzylamine was generally not high. Therefore, the method for modifying the nickel-based catalyst with vanadate, tungstate or molybdate provided by the present invention can effectively improve the catalytic efficiency of the benzonitrile hydrogenation reaction of the nickel-based catalyst.

[0295] Application Example 1

[0296] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds, the method comprising the following steps: dissolving 16 mg of the catalyst provided in Example 1, 5 mmol of 2,4-dimethylbenzonitrile, and 500 μL of aqueous ammonia in 5 mL of methanol solution, adding the mixture into a high-pressure reactor, introducing 2.5 MPa of hydrogen, heating the mixture to 80° C., setting the rotation speed to 800 rpm, reacting for 10 hours, taking 50 μL of the reaction solution, and detecting the yield of the product 2,4-dimethylbenzylamine by gas chromatography.

[0297] Application Example 2

[0298] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by p-chlorobenzonitrile, and the reaction time is reduced to 4 hours; and the yield of the product p-chlorobenzylamine is detected by gas chromatography.

[0299] Application Example 3

[0300] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by p-fluorobenzonitrile, and the reaction time is reduced to 6 hours; and the yield of the product p-chlorobenzylamine is detected by gas chromatography.

[0301] Application Example 4

[0302] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by o-chlorobenzonitrile, and the reaction time is reduced to 4 hours; and the yield of the product o-chlorobenzylamine is detected by gas chromatography.

[0303] Application Example 5

[0304] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by p-methylbenzonitrile, and the reaction time is reduced to 2 hours; and the yield of the product p-methylbenzylamine is detected by gas chromatography.

[0305] Application Example 6

[0306] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by m-methylbenzonitrile, and the reaction time is reduced to 2 hours; and the yield of the product m-methylbenzylamine is detected by gas chromatography.

[0307] Application Example 7

[0308] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by o-methylbenzonitrile, and the reaction time is reduced to 2 hours; and the yield of the product o-methylbenzylamine is detected by gas chromatography.

[0309] Application Example 8

[0310] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by p-methoxybenzonitrile, and the reaction time is reduced to 2 hours; and the yield of the product p-methoxybenzylamine is detected by gas chromatography.

[0311] Application Example 9

[0312] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by o-methoxybenzonitrile, and the reaction time is reduced to 2 hours; and the yield of the product o-methoxybenzylamine is detected by gas chromatography.

[0313] Application Example 10

[0314] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by p-ethylbenzonitrile, and the reaction time is reduced to 2 hours; and the yield of the product p-ethylbenzylamine is detected by gas chromatography.

[0315] Application Example 11

[0316] This application example provides a method for preparing primary amines by catalytic hydrogenation of nitrile compounds. The only difference from Application Example 1 is that 2,4-dimethylbenzonitrile is replaced by p-tert-butylbenzonitrile, and the reaction time is reduced to 4 hours; and the yield of the product p-tert-butylbenzylamine is detected by gas chromatography.

[0317] Test Example 6

[0318] Hydrogenation substrate investigation

[0319] Test sample: the reaction solution provided in Application Examples 1 to 11;

[0320] The test results are shown in Table 7 below:

[0321] Table 7

[0322]

[0323]

[0324] It can be seen from Table 7 that tungstate-modified Ni@WO xThe / C catalyst has excellent hydrogenation performance for different nitrile substrates, and the yield of the corresponding primary amine product reaches about 95%.

[0325] More specifically, by tracking the product yield curves of the hydrogenation of 2,4-dimethylbenzonitrile to 2,4-dimethylbenzylamine catalyzed by the Ni / C catalyst before and after modification, it can be seen that the Ni / C catalyst before modification showed poor activity for the hydrogenation of 2,4-dimethylbenzonitrile and was also poisoned. This is because the product amine has a strong interaction with the metal nickel, which is adsorbed on the surface and blocks the active sites, thus causing the catalyst to be poisoned. The modified Ni@WO x The tungsten oxide coating on the surface of the / C catalyst can not only effectively inhibit the agglomeration of nickel nanoparticles, but also provide a large number of B acid sites to promote hydrogen transfer during the hydrogenation of nitrile compounds, thereby significantly improving the activity of 2,4-dimethylbenzonitrile hydrogenation reaction; at the same time, the presence of a large number of B acid sites makes the product amine protonated to a certain extent, weakening its coordination ability and ensuring that the catalyst is not poisoned during the hydrogenation process. After the modification, the target product ( Figure 5 ).

[0326] Therefore, the method for modifying the nickel-based catalyst provided by the present invention is not only applicable to the modification of various nickel-based catalysts, but also applicable to the hydrogenation of nitrile substrates with different functional groups. It has a wide range of substrate applicability and can effectively improve the catalytic efficiency of the hydrogenation reaction of benzonitrile using a nickel-based catalyst.

[0327] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. Use of a catalyst in catalyzing the hydrogenation of nitrile compounds to prepare primary amines, characterized in that: The catalyst comprises a nickel-based catalyst and a metal oxide; The metal oxide includes any one of tungsten oxide, molybdenum oxide or vanadium oxide, or a combination of at least two of them.

2. The use according to claim 1, characterized in that: The metal oxide forms a coating layer on the surface of the nickel-based catalyst; And / or, the 4f orbital binding energy of the tungsten element in the tungsten oxide is 30 to 42 eV; And / or, the 3d orbital binding energy of the molybdenum element in the molybdenum oxide is 228 to 239 eV; And / or, the 2p orbital binding energy of the vanadium element in the vanadium oxide is 510 to 530 eV; Preferably, the loading amount of the metal oxide accounts for 0.01 to 50 wt % of the total mass of the catalyst.

3. The use according to claim 1, characterized in that: The nickel-based catalyst is selected from any one or a combination of at least two of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals; Preferably, the supported nickel-based catalyst comprises a carrier and nickel nanoparticles supported on the carrier; Preferably, the loading amount of the nickel nanoparticles accounts for 1 to 60 wt % of the total mass of the supported nickel-based catalyst; Preferably, the carrier is selected from any one or a combination of at least two of a carbon carrier, Al2O3, SiO2, MgO, TiO2, ZrO2 or CeO2; Preferably, the carbon carrier is selected from any one of activated carbon, carbon nanotubes, carbon black or mesoporous carbon, or a combination of at least two thereof.

4. The use according to claim 1, characterized in that: The preparation method of the catalyst comprises the following steps: The nickel-based catalyst and a metal precursor are mixed, calcined and reduced to obtain the catalyst; wherein the metal precursor includes any one of a tungsten precursor, a molybdenum precursor or a vanadium precursor, or a combination of at least two thereof.

5. The use according to claim 4, characterized in that: The nickel-based catalyst is selected from any one or a combination of at least two of a supported nickel-based catalyst, a Raney nickel catalyst or nickel nanocrystals; And / or, the tungsten precursor is selected from any one of ammonium metatungstate, ammonium paratungstate, sodium tungstate or ammonium tungstate, or a combination of at least two thereof; and / or, the molybdenum precursor is selected from ammonium tetramolybdate and / or ammonium heptamolybdate; And / or, the vanadium precursor is selected from any one or a combination of at least two of sodium metavanadate, sodium pyrovanadate, ammonium metavanadate or sodium orthovanadate.

6. The use according to claim 4, characterized in that: The mass ratio of the metal precursor to the nickel-based catalyst is (0.01-1):1; Preferably, the calcination is carried out under a protective gas atmosphere; wherein the protective gas is selected from any one of nitrogen, argon or hydrogen, or a combination of at least two thereof; Preferably, the calcination temperature is 100 to 600° C., and the calcination time is 1 to 12 hours; Preferably, the reduction is carried out under a reducing gas atmosphere; wherein the reducing gas is selected from hydrogen or a hydrogen-argon mixture; Preferably, the volume percentage of hydrogen in the hydrogen-argon mixed gas is 1 to 50 vol%; Preferably, the reduction temperature is 100-500° C., and the reduction time is 1-4 hours.

7. The use according to claim 5, characterized in that: The supported nickel-based catalyst is prepared by the following steps: adsorbing a nickel salt precursor onto a carrier, and performing calcination reduction to obtain the supported nickel-based catalyst; Preferably, the supported nickel-based catalyst is prepared by the following steps: (a) dispersing the support in a solvent, mixing with a solution containing a nickel precursor, stirring and drying to obtain a solid phase; (b) calcining and reducing the solid phase to obtain the supported nickel-based catalyst; Preferably, in step (a), the nickel precursor is selected from any one or a combination of at least two of Ni(acac)2, Ni(CH3COO)2, Ni(NO3)2, Ni2SO4 or NiCl2; Preferably, in step (a), the mass ratio of the nickel precursor to the carrier is (0.01-1.5):1; Preferably, in step (b), the calcination reduction is carried out in a hydrogen-argon mixed gas atmosphere; Preferably, the volume percentage of hydrogen in the hydrogen-argon mixed gas is 1 to 50 vol%; Preferably, in step (b), the temperature of the calcination reduction is 100 to 600° C., and the time of the calcination reduction is 1 to 12 hours.

8. A method for preparing primary amines by catalytic hydrogenation of nitrile compounds, characterized in that: The method comprises the following steps: The catalyst, nitrile compound, base and reaction solvent are mixed and contacted with hydrogen to carry out catalytic reaction to obtain primary amine compounds; Wherein, the catalyst comprises the catalyst according to any one of claims 1 to 3, or a catalyst obtained by the method for preparing the catalyst according to any one of claims 4 to 7.

9. The method according to claim 8, characterized in that The structural formula of the nitrile compound is shown in the following formula I: Wherein, R2 and R3 represent any organic functional group substituents at different positions of the benzene ring; Preferably, the substituent is selected from any one or a combination of at least two of H, halogen, C1-C6 straight-chain or branched alkyl, C1-C6 straight-chain or branched alkoxy; Preferably, the nitrile compound is selected from any one of benzonitrile, 2,4-dimethylbenzonitrile, p-chlorobenzonitrile, p-fluorobenzonitrile, o-chlorobenzonitrile, p-bromobenzonitrile, p-methylbenzonitrile, m-methylbenzonitrile, o-methylbenzonitrile, p-methoxybenzonitrile, o-methoxybenzonitrile, p-ethylbenzonitrile or p-tert-butylbenzonitrile; Preferably, the base comprises NH3, preferably aqueous ammonia and / or methanolic ammonia solution; Preferably, the reaction solvent is selected from any one or a combination of at least two of water, methanol, ethanol, acetonitrile, toluene, tetrahydrofuran, γ-butyrolactone, chlorobenzene, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl carbonate, dioxane, n-hexane or cyclohexane.

10. The method according to claim 8, characterized in that The temperature of the catalytic reaction is 40 to 90° C., and the time of the catalytic reaction is 2 to 72 hours; Preferably, the pressure of the hydrogen is 0.5-3 MPa; Preferably, the molar ratio of the nickel element to the nitrile compound in the catalyst is 1:(20-400).

Citation Information

Patent Citations

  • Catalyst for preparing fatty primary amine by fatty nitrile hydrogenation and application thereof

    CN101011661A

  • Method for preparing m-xylylenediamine from m-phthalodinitrile through hydrogenation

    CN103539676A

  • Method for synthesizing benzylamine through continuous catalytic hydrogenation of cyanobenzene

    CN104803856A

  • Catalyst for producing amine by hydrogenating nitrile compound and preparation method and application of catalyst

    CN111195523A

  • Catalyst as well as preparation method and application thereof

    CN117531520A