Green mixed solvent and application thereof in preparation of perovskite layer of perovskite solar cell
By combining green mixed solvents with different boiling points, the problem of slow crystallization of perovskite layer in perovskite solar cells is solved, and the efficient preparation of perovskite solar cells with high energy conversion efficiency is achieved under low temperature and short time conditions, which is improved Process tolerance and stability.
Patent Information
- Application Number
- CN202411283432.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-06
AI Technical Summary
When preparing perovskite layers, the boiling point of solvents such as DMF and DMSO is commonly used, resulting in slow crystallization speed, requiring higher temperature and long-term annealing, making it difficult to adapt to high-throughput roll-to-roll printing technology. And the introduction of low boiling point solvents will affect the stability of the precursor.
A green mixed solvent is used to form a perovskite precursor solution with a boiling point of 150-200°C, a medium boiling point of 100-150°C and a low boiling point solvent with a high stability through rotation Apply or scrape the perovskite layer on the hole transport layer or electron transport layer, and anneale the perovskite layer at a low temperature and short time to prepare the
The perovskite crystallization speed is accelerated, and a forward-reverse perovskite solar cell with high energy conversion efficiency is prepared at lower temperatures and shorter time conditions, which improves process tolerance and stability.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of perovskite solar cells, and in particular relates to a green mixed solvent and an application thereof in preparing a perovskite layer of a perovskite solar cell. Background Art
[0002] Energy, as one of the earliest natural resources used by humans, has promoted the progress of civilized society and the development of the economic field. In the face of the continuous consumption of non-renewable energy and the increasingly severe energy crisis, it is imperative to develop green renewable energy technology. Although traditional solar cells based on inorganic semiconductor materials such as silicon have been commercialized, their production process is complicated, the cost is too high, and there are defects such as inorganic materials are non-degradable and difficult to flexibly process, which limits their application scope. Solar energy, as a green renewable energy source that is inexhaustible, is one of the most promising photovoltaic technologies.
[0003] Perovskite cells are one of many types of solar cells and are a promising green and renewable energy source. However, solvents such as DMF and DMSO are often used to prepare perovskite layers. The high boiling points of solvents such as DMF and DMSO result in slow crystallization of perovskites, which usually require annealing at higher temperatures and for longer periods of time, accompanied by difficult-to-precisely control processing processes such as solvent vapor annealing, which is not conducive to the industrialization of perovskite solar cells prepared using high-throughput roll-to-roll printing technology.
[0004] In order to solve the problem that perovskite crystallization is slow due to high boiling point solvents such as DMF and DMSO, and requires higher and longer temperature annealing, the existing technology usually introduces low boiling point solvents such as ethanol or isopropanol into high boiling point solvents such as DMF and DMSO. However, DMF has poor process tolerance, and mixing with low boiling point solvents will cause the stability of the perovskite precursor solution to deteriorate, and even directly cause the solute (i.e., the raw material for forming the perovskite layer) to precipitate.
[0005] Therefore, developing a solvent with low toxicity and high process tolerance suitable for preparing the perovskite layer of perovskite solar cells has certain market value. Summary of the invention
[0006] In view of the deficiencies in the above-mentioned prior art, a green mixed solvent is provided. By compounding three green solvents with different boiling points, different polarities, different chain lengths, different volatility, and different rigid and flexible chains, a perovskite precursor solution with higher stability can be obtained; when preparing the perovskite layer, the crystallization rate of the perovskite can be accelerated, and annealing can be carried out at a lower temperature and in a shorter time, so as to prepare a positive and negative perovskite solar cell with higher energy conversion efficiency.
[0007] The invention aims to provide a green mixed solvent, which is composed of the following solvents: a high boiling point solvent with a boiling point of 150-200°C, a medium boiling point solvent with a boiling point of 100-150°C and a low boiling point solvent with a boiling point below 100°C.
[0008] The mass ratio of the high boiling point solvent with a boiling point of 150-200°C, the medium boiling point solvent with a boiling point of 100-150°C and the low boiling point solvent with a boiling point below 100°C is 1:3-7:10-15.
[0009] In some embodiments of the present invention, the high boiling point solvent with a boiling point of 150-200° C. is selected from at least one of cyclohexanone and cyclohexanol.
[0010] In some embodiments of the present invention, the medium-boiling-point solvent with a boiling point of 100-150° C. is selected from at least one of n-butyl decanoate and isopentyl isodecanoate.
[0011] In some embodiments of the present invention, the low boiling point solvent having a boiling point lower than 100° C. is selected from at least one of acetone and ethanol.
[0012] Another object of the present invention is to provide a perovskite layer precursor solution, comprising raw materials for forming a perovskite layer and the green mixed solvent.
[0013] In some embodiments of the present invention, the raw materials for forming the perovskite layer include AX raw materials and BX2 raw materials.
[0014] In some embodiments of the present invention, the perovskite has an ABX3 structure.
[0015] In some embodiments of the present invention, the AX source is selected from at least one of CH3NH3X, CH3CH2NH3X, and NH2CH=NH2X.
[0016] In some embodiments of the present invention, the BX2 source is selected from at least one of PbX2 and SnX2.
[0017] In some embodiments of the present invention, the X is selected from at least one of Cl, Br and I.
[0018] In some embodiments of the present invention, the mass ratio of the AX source to the BX2 source is (1-3):1.
[0019] In some embodiments of the present invention, the usage ratio of the raw material for forming the perovskite layer to the green mixed solvent is (200-600) mg: 1 ml.
[0020] Another object of the present invention is to provide a method for preparing a perovskite layer of a perovskite solar cell, comprising the following steps:
[0021] The perovskite layer precursor solution is spin-coated or scraped onto the hole transport layer or the electron transport layer, and annealed to obtain the perovskite layer of the perovskite solar cell.
[0022] In some embodiments of the present invention, the spin coating process is 300-700 r / min for 1-5 s, and then 4000-6000 r / min for 20-40 s.
[0023] In some embodiments of the present invention, the speed of the scraping is 5.5-9.5 mm / s, and the flow rate of the nitrogen knife during the scraping is 20-40 L / min.
[0024] In some embodiments of the present invention, the annealing temperature is 50-100° C. and the time is 1-10 min.
[0025] In some embodiments of the present invention, the thickness of the perovskite layer of the perovskite solar cell is 500-800 nm, including but not limited to 500 nm, 530 nm, 560 nm, 590 nm, 620 nm, 650 nm, 680 nm, 710 nm, 740 nm, 770 nm, and 800 nm.
[0026] In some embodiments of the present invention, the material of the hole transport layer is selected from at least one of polyvinyl carbazole, poly [[9-(1-octylnonyl)-9H-carbazole-2,7-diyl]-2,5-thiophenediyl-2,1,3-benzothiadiazole-4,7-diyl-2,5-thiophenediyl], poly 3-hexylthiophene, and poly [bis(4-phenyl)(4-butylphenyl)amine].
[0027] In some embodiments of the present invention, the thickness of the hole transport layer is 10 to 35 nm, including but not limited to 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, and 35 nm.
[0028] In some embodiments of the present invention, the material of the electron transport layer is selected from PC 61 At least one of BM and BCP.
[0029] In some embodiments of the present invention, the thickness of the electron transport layer is 100-200 nm, including but not limited to 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 145 nm, 150 nm, 155 nm, 160 nm, 165 nm, 170 nm, 175 nm, 180 nm, 185 nm, 190 nm, 195 nm, and 200 nm.
[0030] Another object of the present invention is to provide a perovskite solar cell, including a perovskite layer prepared by the method for preparing a perovskite layer of the perovskite solar cell.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention can obtain a perovskite precursor solution with high stability by compounding a high boiling point solvent with a boiling point of 150 to 200°C, a medium boiling point solvent with a boiling point of 100 to 150°C, and a low boiling point solvent with a boiling point below 100°C; when preparing a perovskite layer, the crystallization rate of the perovskite can be accelerated, and annealing can be performed at a lower temperature and a shorter time, thereby preparing a forward and reverse perovskite solar cell with high energy conversion efficiency.
[0033] (2) The boiling point of the cyclohexanone or cyclohexanol used in the present invention is 150-200°C, with a relatively high boiling point, relatively low polarity, low volatility, and a rigid ring structure; the boiling point of the n-butyl decanoate or isoamyl isodecanoate used is 100-150°C, with a medium boiling point, relatively medium polarity, relatively medium volatility, and a long chain structure; the boiling point of the acetone or ethanol used is below 100°C, with a relatively low boiling point, relatively high polarity, high volatility, and a short chain structure. By compounding green solvents with different boiling points, different polarities, different lengths and short chains, different volatility, and different rigid and flexible chains, a perovskite precursor solution with high stability can be obtained; when preparing the perovskite layer, the perovskite crystallization speed can be accelerated, and annealing can be performed at a relatively low temperature and a relatively short time, so as to prepare a positive and negative perovskite solar cell with a relatively high energy conversion efficiency. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0035] All raw materials of the present invention are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods well known to those skilled in the art.
[0036] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials of conventional purity used in the field of perovskite solar cells.
[0037] The brands and abbreviations of all raw materials of the present invention are conventional brands and abbreviations in the art. Each brand and abbreviation is clear and definite in the field of its related use. Those skilled in the art can purchase them from the market or prepare them by conventional methods according to the brands, abbreviations and corresponding uses.
[0038] The invention provides a green mixed solvent, which consists of the following solvents: a high boiling point solvent with a boiling point of 150-200 DEG C, a medium boiling point solvent with a boiling point of 100-150 DEG C and a low boiling point solvent with a boiling point lower than 100 DEG C.
[0039] The conventional content of the mixed solvent well known to those skilled in the art can be used. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. The mass ratio of the high boiling point solvent with a boiling point of 150-200°C, the medium boiling point solvent with a boiling point of 100-150°C and the low boiling point solvent with a boiling point below 100°C is 1:3-7:10-15, preferably 1:4-6:12-14, and more preferably 1:5:13.
[0040] The high boiling point solvent with a boiling point of 150 to 200° C. is selected from at least one of cyclohexanone and cyclohexanol; the medium boiling point solvent with a boiling point of 100 to 150° C. is selected from at least one of n-butyl decanoate and isoamyl isodecanoate; and the low boiling point solvent with a boiling point lower than 100° C. is selected from at least one of acetone and ethanol.
[0041] The invention provides a perovskite layer precursor solution, comprising a raw material for forming a perovskite layer and the green mixed solvent.
[0042] The present invention has no particular limitation on the raw materials for forming the perovskite layer, and any conventional raw materials for forming the perovskite layer known to those skilled in the art may be used. The raw materials for forming the perovskite layer include AX raw materials and BX2 raw materials.
[0043] The present invention has no particular limitation on the structure and definition of the perovskite, and the structure and definition of the perovskite familiar to those skilled in the art may be used. Those skilled in the art may select and adjust according to actual application conditions, product requirements and quality requirements. The perovskite has an ABX3 structure.
[0044] Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. Among the raw materials for forming the perovskite layer described in the present invention, the AX source is selected from at least one of CH3NH3X, CH3CH2NH3X, and NH2CH=NH2X; the BX2 source is selected from at least one of PbX2 and SnX2; and the X is selected from at least one of Cl, Br and I.
[0045] The present invention has no particular restriction on the ratio of the raw materials for forming the perovskite layer. The conventional ratio for forming the perovskite layer known to those skilled in the art can be used. Those skilled in the art can select and adjust according to the actual application conditions, product requirements and quality requirements. The mass ratio of the AX source to the BX2 source in the present invention is (1-3):1, preferably 2:1.
[0046] The present invention has no particular restrictions on the ratio of the raw materials for forming the perovskite layer and the solvent system, and the conventional ratio familiar to those skilled in the art can be used. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. The usage ratio of the raw materials for forming the perovskite layer and the green mixed solvent in the present invention is (200-600) mg: 1 ml.
[0047] The present invention provides a method for preparing a perovskite layer of a perovskite solar cell, comprising the following steps:
[0048] The perovskite layer precursor solution is spin-coated or scraped onto the hole transport layer or the electron transport layer, and annealed to obtain the perovskite layer of the perovskite solar cell.
[0049] The present invention has no particular limitation on the specific steps of the spin coating, and the conventional steps of preparing the perovskite layer by the spin coating method well known to those skilled in the art can be used. Those skilled in the art can select and adjust according to the actual production situation, product requirements and quality requirements. In order to further improve the performance of the perovskite layer, the specific steps of the spin coating of the present invention are preferably first rotating at a low speed and then rotating at a high speed. The spin coating process of the present invention is 300-700 r / min for 1-5s, then 4000-6000 r / min for 20-40s, preferably 400-600 r / min for 1-5s, then 4500-5500 r / min for 20-40s.
[0050] The present invention has no special restrictions on the specific steps of the scraping coating. The conventional steps of preparing the perovskite layer by the scraping coating method well known to those skilled in the art can be used. Those skilled in the art can select and adjust according to the actual production situation, product requirements and quality requirements. In order to further improve the performance of the perovskite layer, the scraping speed of the present invention is 5.5-9.5 mm / s, and the nitrogen knife flow rate during the scraping coating process is 20-40 L / min. Preferably, the scraping speed is 6-8 mm / s, and the nitrogen knife flow rate during the scraping coating process is 25-35 L / min.
[0051] In the present invention, due to the use of a specific solvent system, the present invention can anneal at a lower temperature and in a shorter time to prepare a positive and negative perovskite solar cell with a higher energy conversion efficiency. In order to complete and optimize the preparation method, after the spin coating or scraping coating described in the present invention, an annealing step may be included, and a low-temperature annealing step is more preferably included. The annealing temperature of the present invention is 50 to 100°C and the time is 1 to 10 minutes.
[0052] The present invention has no particular limitation on the thickness of the perovskite layer, and the conventional perovskite layer thickness for forming a perovskite solar cell known to those skilled in the art can be used. Those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. The thickness of the perovskite layer of the perovskite solar cell of the present invention is 500-800nm, including but not limited to 500nm, 530nm, 560nm, 590nm, 620nm, 650nm, 680nm, 710nm, 740nm, 770nm, and 800nm.
[0053] The present invention has no particular restriction on the selection of the hole transport layer, and a conventional hole transport layer for forming a perovskite solar cell known to those skilled in the art can be used. Those skilled in the art can select and adjust it according to the actual application, product requirements and quality requirements. The material of the hole transport layer of the present invention is selected from at least one of polyvinyl carbazole, poly [[9-(1-octylnonyl)-9H-carbazole-2,7-diyl]-2,5-thiophenediyl-2,1,3-benzothiadiazole-4,7-diyl-2,5-thiophenediyl], poly 3-hexylthiophene, and poly [bis (4-phenyl) (4-butylphenyl) amine], preferably poly 3-hexylthiophene.
[0054] The present invention has no particular limitation on the thickness of the hole transport layer, and the conventional hole transport thickness for forming perovskite solar cells known to those skilled in the art can be used. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. The thickness of the hole transport layer of the present invention is 10 to 35 nm, including but not limited to 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, and 35 nm.
[0055] The present invention has no particular restriction on the selection of the electron transport layer. A conventional electron transport layer for forming a perovskite solar cell known to those skilled in the art can be used. Those skilled in the art can select and adjust the material according to the actual application, product requirements and quality requirements. The material of the electron transport layer of the present invention is selected from PC 61 At least one of BM and BCP.
[0056] The present invention has no particular limitation on the thickness of the electron transport layer, and the conventional electron transport layer thickness for forming perovskite solar cells known to those skilled in the art can be used. Those skilled in the art can select and adjust according to actual application conditions, product requirements and quality requirements. The thickness of the electron transport layer of the present invention is 100-200nm, including but not limited to 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm, 140nm, 145nm, 150nm, 155nm, 160nm, 165nm, 170nm, 175nm, 180nm, 185nm, 190nm, 195nm, and 200nm.
[0057] The present invention also provides a perovskite solar cell, comprising a perovskite layer prepared by the method for preparing the perovskite layer of the perovskite solar cell.
[0058] The present invention has no particular limitation on the definition and structure of the perovskite solar cell, and the definition and structure of conventional perovskite solar cells familiar to those skilled in the art may be used. Those skilled in the art may select and adjust according to actual application conditions, product requirements and quality requirements. The perovskite solar cell of the present invention is preferably a perovskite solar cell with a flat heterojunction structure (planar structure), which may be a NIP structure or a PIN structure. The perovskite solar cell further includes a transparent substrate layer, a hole transport layer, an electron transport layer, a hole blocking layer and a metal electrode layer.
[0059] The present invention has no special limitation on the transparent substrate layer, and any conventional transparent substrate layer for forming perovskite solar cells known to those skilled in the art may be used. Those skilled in the art may select and adjust the transparent substrate layer according to actual application conditions, product requirements and quality requirements. The transparent substrate layer of the present invention is transparent conductive glass ITO or FTO.
[0060] The present invention has no particular limitation on the hole blocking layer, and any conventional hole blocking layer for forming a perovskite solar cell known to those skilled in the art may be used. Those skilled in the art may select and adjust the hole blocking layer according to actual application conditions, product requirements and quality requirements. The material of the hole blocking layer of the present invention is selected from BCP.
[0061] The present invention has no special limitation on the metal electrode layer, and any conventional metal electrode layer for forming a perovskite solar cell known to those skilled in the art may be used. Those skilled in the art may select and adjust the metal electrode layer according to actual application conditions, product requirements and quality requirements. The material of the metal electrode layer of the present invention is selected from silver or gold.
[0062] The present invention has no particular limitation on the square resistance of the transparent substrate layer. The square resistance of a conventional transparent substrate layer for forming a perovskite solar cell known to those skilled in the art can be used. Those skilled in the art can select and adjust it according to actual application conditions, product requirements and quality requirements. The square resistance of the transparent substrate layer of the present invention is ≤80Ω.
[0063] The present invention has no particular limitation on the thickness of the hole blocking layer, and the conventional hole blocking layer thickness for forming perovskite solar cells known to those skilled in the art can be used. Those skilled in the art can select and adjust the thickness according to actual application conditions, product requirements and quality requirements. The thickness of the hole blocking layer in the present invention is 5 to 10 nm.
[0064] The present invention has no particular limitation on the thickness of the metal electrode layer, and the conventional metal electrode layer thickness for forming perovskite solar cells known to those skilled in the art can be used. Those skilled in the art can select and adjust the thickness according to actual application conditions, product requirements and quality requirements. The thickness of the metal electrode layer of the present invention is 50 to 200 nm.
[0065] The present invention provides a method for preparing the perovskite solar cell, comprising the following steps:
[0066] A hole transport layer, a perovskite layer, an electron transport layer, a hole blocking layer and a metal electrode layer are sequentially stacked on the transparent base layer.
[0067] The present invention provides a method for preparing the perovskite solar cell, comprising the following steps:
[0068] A hole blocking layer, an electron transport layer, a perovskite layer, a hole transport layer and a metal electrode layer are sequentially stacked on the transparent base layer.
[0069] Example 1
[0070] This embodiment provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the specific implementation steps are as follows:
[0071] S1. Cleaning of transparent substrate layer: first take out the ITO transparent conductive glass with a square resistance of ≤80Ω, tear off the plastic protective film on the surface, first gently wipe the surface oil with detergent, then ultrasonically clean it in a low concentration of detergent solution, deionized water, and isopropanol for 15 minutes respectively, finally blow dry the isopropanol on the ITO surface with nitrogen, and pack it in a box for later use;
[0072] S2. Preparation of hole transport layer (P3HT): P3HT was prepared into a precursor solution of 0.2 mg / mL, the solvent was chlorobenzene, the cleaned ITO was first placed in an ultraviolet ozone cleaner for surface hydrophilic treatment, and then the precursor solution of P3HT was sucked out with a pipette and evenly covered on the surface of ITO, first spin-coated at 500 rpm / min for 3 seconds, then spin-coated at 3000 rpm / min for 20 seconds, and the solvent was dried to form a hole transport layer with a thickness of 10 to 35 nm;
[0073] S3. Preparation of a perovskite layer precursor solution: 2 g of lead iodide and methyl iodide in a mass ratio of 1:1 were dissolved in 10 ml of cyclohexanone, n-butyl decanoate and acetone in a mass ratio of 1:3:15 to prepare a mixed solution of lead iodide and methyl iodide, i.e., a perovskite layer precursor solution;
[0074] S4. Preparation of perovskite layer: The FAPbI3 system perovskite precursor solution is sucked out with a pipette and evenly covered on the surface of the hole transport layer, first spin-coated at 300-700 r / min for 1-5 s, then spin-coated at 4000-6000 r / min for 20-40 s to form a perovskite layer, and then annealed at 100°C on a hot stage for 10 min to form a perovskite layer with a thickness of 500-800 nm;
[0075] S5. Preparation of electron transport layer: weigh 20 mg PC 61 BM was added with 1 mL of chlorobenzene to prepare a precursor solution of the electron transport layer, and the precursor solution of the electron transport layer was deposited on the surface of the perovskite layer by spin coating (first at 500 rpm / min for 3 s, then at 2500 rpm / min for 20 s) to form an electron transport layer with a thickness of 100 to 200 nm;
[0076] S6. Preparation of hole blocking layer: 8 mg BCP was weighed, 16 mL isopropanol was added to prepare a precursor solution, and then the prepared precursor solution was sucked out with a pipette and evenly covered on the surface of the electron transport layer, first spin-coated at 100 rpm / min for 3 s, then spin-coated at 5000 rpm / min for 20 s, and the solvent was dried to form a hole blocking layer with a thickness of 5 to 10 nm;
[0077] S7. Deposition of metal electrode layer: 100 nm thick Ag film was evaporated under high vacuum at an evaporation rate of: 20nm was deposited under the conditions, and then Under the conditions, it is deposited on the surface of the hole blocking layer, with a deposition thickness of 50 to 200 nm and a deposition area of about 0.07 cm 2 .
[0078] Example 2
[0079] This embodiment provides a perovskite solar cell, and the specific cell structure is ITO / polyvinyl carbazole / perovskite layer / PCBM / BCP / Ag. The difference from the embodiment 1 is only that steps S2, S3 and S4 are different. P3HT in step S2 is replaced by polyvinyl carbazole. The specific implementation steps of steps S3 and S4 are as follows:
[0080] S3. Preparation of a perovskite layer precursor solution: 6 g of lead iodide and methyl iodide in a mass ratio of 3:1 were dissolved in 10 ml of cyclohexanone, isoamyl isodecanoate and acetone in a mass ratio of 1:7:10 to obtain a mixed solution of lead iodide and methyl iodide, i.e., a perovskite layer precursor solution;
[0081] S4. Preparation of perovskite layer: Use a scraper coater to place the hole transport layer prepared in S2 under the scraper, take the perovskite layer precursor prepared in S3 and inject it into the scraper gap, the scraping speed is 5.5-9.5 mm / s, the nitrogen knife flow rate during the scraping process is 20-40 L / min, and a perovskite layer is formed, and then annealed on a hot stage at 50°C for 1 min to form a perovskite layer with a thickness of 500-800 nm.
[0082] Example 3
[0083] This embodiment provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the difference from the embodiment 1 is only that step S3 is different. The specific implementation steps of step S3 are as follows:
[0084] S3. Preparation of perovskite layer precursor solution: 2 g of lead iodide and methyl iodide in a mass ratio of 1:1 are dissolved in 10 ml of cyclohexanol, n-butyl decanoate and acetone in a mass ratio of 1:3:15 to obtain a mixed solution of lead iodide and methyl iodide, i.e., the perovskite layer precursor solution.
[0085] Example 4
[0086] This embodiment provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the difference from the embodiment 1 is only that step S3 is different. The specific implementation steps of step S3 are as follows:
[0087] S3. Preparation of perovskite layer precursor solution: 2 g of lead iodide and methyl iodide in a mass ratio of 1:1 are dissolved in 10 ml of cyclohexanol, n-butyl decanoate and ethanol in a mass ratio of 1:3:15 to obtain a mixed solution of lead iodide and methyl iodide, i.e., the perovskite layer precursor solution.
[0088] Comparative Example 1
[0089] This comparative example provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the only difference from Example 1 is that step S3 is different. The specific implementation steps of step S3 are as follows:
[0090] S3. Preparation of perovskite layer precursor solution: Dissolve 2 g of lead iodide and iodomethylamine in a mass ratio of 1:1 in 10 ml of cyclohexanol to prepare a mixed solution of lead iodide and iodomethylamine, i.e., the perovskite layer precursor solution.
[0091] Comparative Example 2
[0092] This comparative example provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the only difference from Example 1 is that step S3 is different. The specific implementation steps of step S3 are as follows:
[0093] S3. Preparation of perovskite layer precursor solution: Dissolve 2 g of lead iodide and iodomethylamine in a mass ratio of 1:1 in 10 ml of cyclohexanone to prepare a mixed solution of lead iodide and iodomethylamine, i.e., the perovskite layer precursor solution.
[0094] Comparative Example 3
[0095] This comparative example provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the only difference from Example 1 is that step S3 is different. The specific implementation steps of step S3 are as follows:
[0096] S3. Preparation of perovskite layer precursor solution: Dissolve 2 g of lead iodide and methyl iodide in a mass ratio of 1:1 in 10 ml of n-butyl decanoate to prepare a mixed solution of lead iodide and methyl iodide, i.e., the perovskite layer precursor solution.
[0097] Comparative Example 4
[0098] This comparative example provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the only difference from Example 1 is that step S3 is different. The specific implementation steps of step S3 are as follows:
[0099] S3. Preparation of perovskite layer precursor solution: Dissolve 2 g of lead iodide and iodomethylamine in a mass ratio of 1:1 in 10 ml of isoamyl isodecanoate to prepare a mixed solution of lead iodide and iodomethylamine, i.e., the perovskite layer precursor solution.
[0100] Comparative Example 5
[0101] This comparative example provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the only difference from Example 1 is that step S3 is different. The specific implementation steps of step S3 are as follows:
[0102] S3. Preparation of perovskite layer precursor solution: Dissolve 2 g of lead iodide and iodomethylamine in a mass ratio of 1:1 in 10 ml of ethanol to prepare a mixed solution of lead iodide and iodomethylamine, i.e., the perovskite layer precursor solution.
[0103] Comparative Example 6
[0104] This comparative example provides a perovskite solar cell, the specific cell structure is ITO / P3HT / perovskite layer / PCBM / BCP / Ag, and the only difference from Example 1 is that step S3 is different. The specific implementation steps of step S3 are as follows:
[0105] S3. Preparation of perovskite layer precursor solution: Dissolve 2 g of lead iodide and methyl iodine in a mass ratio of 1:1 in 10 ml of acetone to prepare a mixed solution of lead iodide and methyl iodine, i.e., the perovskite layer precursor solution.
[0106] Performance test: The perovskite solar cells of Examples 1 to 4 and Comparative Examples 1 to 6 were tested for performance. The JV characteristic curves of the devices were measured using a Keithley 2440 light source under a simulated AM1.5G spectrum. A solar simulator (Newport, 91160) was used to calibrate the light intensity using a standard silicon solar cell device from NREL. The effective measurement area was 0.07 cm 2 , under reverse and forward bias scans, the scan rate was 100mV / s and the bias range was from -0.2V to 1.2V.
[0107] Table 1. Performance tests of perovskite solar cells of Examples 1 to 4 and Comparative Examples 1 to 6.
[0108] sample Voc(V) <![CDATA[Jsc(mA / cm 2 )]]> FF(%) PCE(%) Example 1 1.03 23.12 76.58 18.23 Example 2 1.04 23.25 76.74 18.56 Example 3 1.04 23.44 78.56 19.15 Example 4 1.05 23.38 79.83 19.60 Comparative Example 1 0.94 20.38 62.34 11.94 Comparative Example 2 0.91 20.42 63.62 11.82 Comparative Example 3 0.93 19.92 64.12 11.88 Comparative Example 4 0.90 19.76 65.09 11.58 Comparative Example 5 0.97 22.01 70.66 15.09 Comparative Example 6 0.98 21.85 70.52 15.10
[0109] As can be seen from Table 1, the energy conversion efficiency of the perovskite solar cells prepared in Examples 1 to 4 of the present invention is high. Compared with Examples 1 to 2, the energy conversion efficiency of the perovskite solar cells in Examples 3 to 4 is higher. The possible reason is that the green mixed solvents in Examples 3 to 4 contain active hydrogen, which increases the interaction between the green mixed solvent and the perovskite raw material, thereby improving the energy conversion efficiency of the perovskite solar cell. Comparative Examples 1 to 6 use a single green solvent, and the energy conversion efficiency of the perovskite solar cells obtained therefrom is lower than that of Examples 1 to 4 of the present application.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that after reading the specification of this application, the technicians can still modify or replace the specific implementation mode of the present invention with equivalents, but these modifications or changes do not deviate from the scope of protection of the pending claims of the present application.
Claims
1. A green mixed solvent, characterized in that: The solvent is composed of the following solvents: a high boiling point solvent with a boiling point of 150-200°C, a medium boiling point solvent with a boiling point of 100-150°C, and a low boiling point solvent with a boiling point below 100°C.
2. The green mixed solvent as claimed in claim 1, characterized in that: The mass ratio of the high boiling point solvent with a boiling point of 150-200°C, the medium boiling point solvent with a boiling point of 100-150°C and the low boiling point solvent with a boiling point below 100°C is 1:3-7:10-15.
3. The green mixed solvent according to claim 1, characterized in that: The high boiling point solvent with a boiling point of 150-200° C. is selected from at least one of cyclohexanone and cyclohexanol; The medium boiling point solvent with a boiling point of 100-150° C. is selected from at least one of n-butyl decanoate and isoamyl isodecanoate; The low boiling point solvent with a boiling point lower than 100° C. is selected from at least one of acetone and ethanol.
4. A perovskite layer precursor solution, characterized in that: Comprising raw materials for forming a perovskite layer and the green mixed solvent according to any one of claims 1 to 3; The raw materials for forming the perovskite layer include AX raw materials and BX2 raw materials; The perovskite has an ABX3 structure; The AX source is selected from at least one of CH3NH3X, CH3CH2NH3X, and NH2CH=NH2X; The BX2 source is selected from at least one of PbX2 and SnX2; The X is selected from at least one of Cl, Br and I.
5. The perovskite layer precursor solution according to claim 4, characterized in that: The mass ratio of the AX source to the BX2 source is (1-3):1; The usage ratio of the raw material for forming the perovskite layer to the green mixed solvent according to any one of claims 1 to 3 is (200 to 600) mg: 1 ml.
6. A method for preparing a perovskite layer of a perovskite solar cell, characterized in that: The following steps are involved: The perovskite layer precursor solution according to any one of claims 4 to 5 is spin-coated or scraped onto the hole transport layer or the electron transport layer, and annealed to obtain the perovskite layer of the perovskite solar cell.
7. The method for preparing a perovskite layer of a perovskite solar cell according to claim 6, characterized in that: The spin coating process is 300-700 r / min for 1-5 s, and then 4000-6000 r / min for 20-40 s; The speed of the scraping is 5.5-9.5 mm / s, and the flow rate of the nitrogen knife during the scraping is 20-40 L / min.
8. The method for preparing a perovskite layer of a perovskite solar cell according to claim 6, characterized in that: The annealing temperature is 50-100° C. and the annealing time is 1-10 min.
9. The method for preparing a perovskite layer of a perovskite solar cell according to claim 6, characterized in that: The thickness of the perovskite layer of the perovskite solar cell is 500-800 nm.