Preparation method of antistatic fluoroelastomer composition
By modifying the dispersion and emulsion polymerization of graphene oxide nanoparticles in fluoroelastomer and combining with the bridge structure containing carbon fillers, the problem of poor electrostatic accumulation and dispersion of fluoroelastomer is solved, and efficient anti-static and mechanical properties are achieved promote.
Patent Information
- Application Number
- CN202411245282.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-14
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
Fluoroelastomers are prone to electrostatic accumulation in semiconductor manufacturing. Existing antistatic agents interact with other additives or are not suitable for high-energy plasma etching environments. The poor dispersion of graphene oxide in fluoroelastomers affects performance.
By ultrasonic dispersing graphene oxide nanoparticles in a mixed solution of perfluorosilane and hydrogen fluoride in ethanol water, hydrophobically modified graphene oxide nanoparticles are formed, and grinded and emulsion polymerized in fluoroether oil, copolymerized fluoromonomer is added. With the vulcanized point monomer, a conductive network is formed, and a bridge structure is formed during the thin-through mixing process by combining carbon-containing fillers to improve anti-static properties.
The antistatic effect without metal impurities in the semiconductor process is achieved, the cleanliness and antistatic properties of the fluoroelastomer are improved, graphene oxide agglomeration is avoided, and the conductive network and mechanical properties are enhanced.
Smart Images

Figure CN119080990A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of fluororubber, and in particular to a method for preparing an antistatic fluoroelastomer composition. Background Art
[0002] Fluoroelastomer is a copolymer of tetrafluoroethylene (TFE) and at least one monomer such as vinylidene fluoride (VDF), perfluorophenoxypropyl vinyl ether (PTVE) and perfluoroalkyl vinyl ether (PAVE). Similar to polytetrafluoroethylene (PTFE), the hydrogen atoms on the molecular chain of fluoroelastomer are partially or completely replaced by fluorine atoms, making it have good heat resistance and chemical resistance.
[0003] However, fluoroelastomer is a non-polar elastomer with a relatively high volume resistivity, and is an electrical insulating material. When the surface of fluororubber is subjected to friction caused by movement and stress, it is easy to cause charge accumulation and form static electricity. In the semiconductor process, some moving points need to be sealed with fluororubber with antistatic function, such as the chuck used to fix the mask and wafer in the lithography machine, and its sealing material needs to have antistatic function.
[0004] Although adding traditional antistatic agents can fundamentally prevent static electricity, they may interact with other additives in fluororubber or be unsuitable for the corrosive high-energy plasma etching environment in semiconductor processes.
[0005] Using conductive fillers as antistatic agents is an option, so that the fluoroelastomer composition can achieve antistatic effect while maintaining other excellent properties.
[0006] CN114085477B discloses an oil-resistant conductive fluororubber, a preparation method and an application thereof. In the preparation method, a fluororubber compound and a nitrile rubber compound are first prepared, the nitrile rubber compound is freeze-ground into powder, sieved, and mixed with carbon nanotubes to obtain a mixed powder, the mixed powder is mixed with the fluororubber compound, and the obtained compound is vulcanized to obtain an oil-resistant conductive fluororubber that can be used as a shape memory material.
[0007] CN113105703A discloses a modified conductive fluororubber, a preparation method and a conductive medium-resistant fluororubber sealing ring. The modified conductive fluororubber contains the following components in parts by mass: 80-120 parts of fluororubber, 0-20 parts of dispersant, 0-10 parts of acid absorber, 5-20 parts of plasticizer, 11-50 parts of reinforcing carbon black, 11-50 parts of conductive carbon black, 0-10 parts of accelerator, 11-50 parts of nano-additive and 0-10 parts of vulcanizer. The prepared modified conductive fluororubber has excellent temperature resistance and medium resistance.
[0008] CN115594986A discloses a highly conductive fluororubber seal ring for lithium batteries and a preparation method thereof. A lignin-based flame retardant is first synthesized, and then polydopamine is loaded on the surface of the lignin flame retardant under alkaline conditions by interfacial polymerization to prepare polydopamine microcapsules, which solves the agglomeration problem caused by direct blending of the lignin-based flame retardant and fluororubber, not only improving the flame retardant properties of the fluororubber, but also enhancing the tensile strength of the fluororubber.
[0009] Graphene oxide (GO) is characterized by rich surface functional groups and high activity. Graphene oxide flakes are the product of graphite powder after chemical oxidation and exfoliation. Graphene oxide is a single atomic layer that can be expanded to tens of microns in lateral dimensions at any time. Graphene oxide can be regarded as a non-traditional soft material with the characteristics of polymers, colloids, films, and amphiphilic molecules.
[0010] The factor that affects the efficiency of graphene oxide filler is mainly its dispersibility. Dispersibility is related to the surface activity and surface structure of graphene oxide. The smaller the particle size, the more complex its surface chemical properties, the higher the surface energy, the more it tends to agglomerate and is difficult to disperse, which has an adverse effect on the final performance of fluoroelastomer composites. Therefore, in order to obtain fluoroelastomer composites with excellent performance, it is extremely critical to improve the dispersion of graphene oxide in the fluoroelastomer matrix and its interfacial interaction with the matrix.
[0011] Based on this, a new technical solution is needed. Summary of the invention
[0012] In view of this, the embodiments of this specification provide a method for preparing an antistatic fluoroelastomer composition to improve the antistatic effect of the fluoroelastomer composition.
[0013] The embodiments of this specification provide the following technical solutions: a method for preparing an antistatic fluoroelastomer composition, comprising:
[0014] S1: placing graphene oxide nanoparticles in a mixed solution of ethanol and water containing perfluorosilane and hydrogen fluoride for ultrasonic dispersion, and separating, washing and drying the solution after ultrasonic dispersion to obtain hydrophobically modified graphene oxide nanoparticles;
[0015] S2: grinding the hydrophobically modified graphene oxide nanoparticles in fluoroether oil and ultrasonically dispersing them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension;
[0016] S3: firstly subjecting 10-30% of the total weight of hydrophobically modified graphene oxide fluoroether oil suspension to emulsion polymerization with copolymerized fluorine-containing monomer and vulcanization point monomer, and then adding the remaining part of the graphene oxide fluoroether oil suspension dropwise to obtain a fluoroelastomer composite emulsion containing modified graphene oxide, wherein the graphene oxide nanoparticles are 5-15wt% of the weight of the copolymerized fluorine-containing monomer;
[0017] S4: washing, drying and thinning the fluoroelastomer composite emulsion after coagulation to obtain a fluoroelastomer;
[0018] S5: thin-pass, knead, compression-form and secondary-vulcanize the fluoroelastomer to obtain a fluoroelastomer composition, and add a carbon-containing filler during the thin-pass and kneading process, wherein the carbon-containing filler is 5-10wt% of the mass of the copolymerized fluorine-containing monomer.
[0019] Optionally, the copolymerized fluorine-containing monomer is composed of a copolymer formed by tetrafluoroethylene and at least one of the following monomers: vinylidene fluoride, hexafluoropropylene, perfluorophenoxypropyl vinyl ether and perfluoroalkyl vinyl ether.
[0020] Optionally, the content of tetrafluoroethylene in the copolymerized fluorine-containing monomer is 31-60 wt %.
[0021] Optionally, the graphene oxide nanoparticles have a thickness of 1-6 nm and a sheet diameter of 1-5 μm.
[0022] Optionally, the perfluorosilane is heptadecafluorodecyltrimethoxysilane or perfluorodecyltriethoxysilane.
[0023] Optionally, the fluoroether oil is a mixture of CF3CF2CF2O(CF(CF3)CF2O)nCF=CF2, n=1-5 and CF3O(CF2O)mCF=CF2, m=1-6, and the mass ratio of CF3CF2CF2O(CF(CF3)CF2O)nCF=CF2 and CF3O(CF2O)mCF=CF2 is 1:1-2.
[0024] Optionally, the mass ratio of the hydrophobically modified graphene oxide nanoparticles to the fluoroether oil is 1:1-2.
[0025] Optionally, the vulcanization point monomer is chlorotrifluoroethylene, vinyl chloride, propylene, isobutylene or 3-bromoperfluoro(propyl vinyl) ether, and the amount of the vulcanization point monomer added is 0.5-5wt% of the mass of the copolymerized fluorine-containing monomer.
[0026] Optionally, the carbon-containing filler includes one or more of graphene, carbon nanotubes and carbon black.
[0027] Optionally, the compression molding conditions are compression pressure 8-12 MPa, compression temperature 160-175° C., and compression time 5-16 min; and the secondary vulcanization conditions are vulcanization temperature 200-220° C., and vulcanization time 10-24 hr.
[0028] Optionally, in S3, the temperature of the emulsion polymerization is 80-120°C, and during the process of adding the remaining portion of the graphene oxide fluoroether oil suspension, the reaction temperature increases by 20-50°C.
[0029] Optionally, in S1, the perfluorosilane solution contains 0.5-4wt% perfluorosilane, 0.5-4wt% hydrogen fluoride, 80-85wt% ethanol, and the rest is water.
[0030] Compared with the prior art, the at least one technical solution adopted in the embodiments of this specification can achieve the following beneficial effects:
[0031] The fluoroelastomer composition prepared in the present application is used to seal antistatic points in the photolithography or etching process in the semiconductor manufacturing process. Since the elastomer composition does not contain metal ions, the elastomer does not contain metal impurities after etching during the photolithography or etching process. The graphene is oxidized into carbon dioxide and escapes from the reaction chamber with the reaction gas, which will not cause pollution to the reaction chamber.
[0032] Hydrofluoric acid provides acidic conditions to promote the hydrolysis of perfluorosilane. After the perfluorosilane is hydrolyzed, low molecular alcohol is released. The active silanol generated thereby forms a self-assembled monomolecular fluorine silicon film layer on the surface of graphene oxide nanoparticles, so that the graphene oxide nanoparticles have extremely low surface energy and excellent hydrophobic properties, and reduce the agglomeration of graphene oxide nanoparticles. During the grinding process, the fluoroether oil fully wraps the hydrophobic graphene oxide nanoparticles, so that the hydrophobic graphene oxide nanoparticles are dispersed in the micelles formed by the emulsion polymerization reaction of the copolymerized fluorine-containing monomer and the vulcanization point monomer. The graphene oxide nanoparticles form a conductive network in the fluoroelastomer matrix, giving full play to its antistatic effect, and also play a filler reinforcement role;
[0033] The hydrofluoric acid hydrolysis generates fluoride ions, which react with the hydroxyl groups of graphene oxide, thereby increasing the compatibility between graphene oxide and perfluorosilane and copolymerized fluorine-containing monomers, so that the graphene oxide and copolymerized fluorine-containing monomers are fully mixed to form a conductive network in the fluoroelastomer;
[0034] The graphene oxide added in the process of emulsion polymerization forms a fluoroelastomer composite emulsion with the copolymerized fluorine-containing monomer, and the carbon-containing filler is added in the process of thin-pass and mixing, so that the carbon-containing filler and the graphene oxide form a bridge structure, thereby improving the antistatic performance of the fluoroelastomer composition;
[0035] The present application directly disperses the hydrophobically modified graphene oxide nanoparticles into the micelles formed by the emulsion polymerization reaction of copolymerized fluorine-containing monomers and vulcanization point monomers by means of a fluoroether oil suspension. Compared with purchasing hydrophobic graphene from outside, it eliminates more surfactants and other stabilizers for maintaining the stability of the graphene, eliminates the interference of stabilizers such as surfactants, and improves the cleanliness of the fluoroelastomer composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 It is a process flow chart of a method for preparing an antistatic fluoroelastomer composition of the present application. DETAILED DESCRIPTION
[0038] The embodiments of the present application are described in detail below with reference to the accompanying drawings.
[0039] The following describes the implementation methods of the present application through specific specific examples, and those skilled in the art can easily understand other advantages and effects of the present application from the content disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The present application can also be implemented or applied through other different specific implementation methods, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application. It should be noted that, in the absence of conflict, the features in the following embodiments and embodiments can be combined with each other. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present application.
[0040] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein can be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present application, it should be understood by those skilled in the art that an aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.
[0041] Additionally, in the following description, specific details are provided to facilitate a thorough understanding of the examples. However, it will be understood by those skilled in the art that the examples can be practiced without these specific details.
[0042] Based on this, the present specification proposes a method for preparing an antistatic fluoroelastomer composition, such as Figure 1As shown, the following steps are included:
[0043] Step 1: ultrasonically dispersing graphene oxide nanoparticles in a mixed solution of ethanol and water containing perfluorosilane and hydrogen fluoride, and separating, washing and drying the solution after ultrasonic dispersion to obtain hydrophobically modified graphene oxide nanoparticles;
[0044] Step 2: grinding the hydrophobically modified graphene oxide nanoparticles in fluoroether oil and ultrasonically dispersing them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension;
[0045] Step 3: firstly subjecting 10-30% of the total weight of the hydrophobically modified graphene oxide fluoroether oil suspension to emulsion polymerization with the copolymerized fluorine-containing monomer and the vulcanization point monomer, and then adding the remaining part of the graphene oxide fluoroether oil suspension dropwise to obtain a fluoroelastomer composite emulsion containing modified graphene oxide, wherein the graphene oxide nanoparticles are 5-15wt% of the weight of the copolymerized fluorine-containing monomer;
[0046] Step 4: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0047] Step 5: Thin-pass, knead, compression mold and secondary vulcanize the fluoroelastomer to obtain a fluoroelastomer composition, and add a carbon-containing filler during the thin-pass and kneading process, wherein the carbon-containing filler is 5-10wt% of the mass of the copolymerized fluorine-containing monomer.
[0048] In step 3, the copolymerized fluorine-containing monomer is composed of a copolymer formed by tetrafluoroethylene and at least one of the following monomers: vinylidene fluoride, hexafluoropropylene, perfluorophenoxypropyl vinyl ether and perfluoroalkyl vinyl ether, wherein the content of tetrafluoroethylene is 31-60 wt%.
[0049] In step 1, the thickness of the graphene oxide nanoparticles is 1-6 nm, the diameter of the flakes is 1-5 μm, and the graphene oxide nanoparticles are 5-25 wt% of the mass of the copolymerized fluorine-containing monomer.
[0050] In step 1, the perfluorosilane is heptadecafluorodecyltrimethoxysilane or perfluorodecyltriethoxysilane. The perfluorosilane solution contains 0.5-4wt% perfluorosilane, 0.5-4wt% hydrogen fluoride, 80-85wt% ethanol, and the rest is water, which is deionized water in this application.
[0051] In step five, the carbon-containing filler includes one or more of graphene, carbon nanotubes and carbon black.
[0052] In step 2, the fluoroether oil is a mixture of CF3CF2CF2O(CF(CF3)CF2O)nCF=CF2, n=1-5 and CF3O(CF2O)mCF=CF2, m=1-6, and the mass ratio of CF3CF2CF2O(CF(CF3)CF2O)nCF=CF2 to CF3O(CF2O)mCF=CF2 is 1:1-2. The mass ratio of the hydrophobically modified graphene oxide nanoparticles to the fluoroether oil is 1:1-2.
[0053] In step 3, the vulcanization point monomer is selected from chlorotrifluoroethylene, vinyl chloride, propylene, isobutylene or 3-bromoperfluoro(propyl vinyl) ether; the amount of the vulcanization point monomer added is 0.5-5wt% of the mass of the copolymerized fluorine-containing monomer.
[0054] In step three, the temperature of the emulsion polymerization is 80-120° C. During the addition of the remaining portion of the graphene oxide fluoroether oil suspension, the reaction temperature is increased by 20-50° C. and the stirring speed is reduced.
[0055] In step 5, the compression molding conditions are compression pressure 8-12 MPa, compression temperature 160-175° C., and compression time 5-16 min; the secondary vulcanization conditions are vulcanization temperature 200-220° C., and vulcanization time 10-24 hr.
[0056] In step one, an initiator and a chain transfer agent are added during the emulsion polymerization process. The initiator may be potassium persulfate or sodium persulfate, and the chain transfer agent may be 1,4-diiodobutane or 1,6-diiodohexane. The types and amounts of the initiator and chain transfer agent in this application are conventional amounts in the industry and are not particularly limited herein.
[0057] The coagulation, washing and drying of the polymer emulsion described in the present application are carried out using conventional processes in the art.
[0058] In step five, a vulcanizing agent, a vulcanizing aid and an acid absorber are added during the thin mixing process. The vulcanizing agent can be 2,5-dioxy-2,5-bis(1-butylated)hexane, the vulcanizing aid can be triallyl cyanurate, and the acid absorber can be zinc oxide or magnesium oxide. In this application, the vulcanizing agent, the vulcanizing aid and the acid absorber are conventional types and amounts in the industry and are not particularly limited herein.
[0059] Example 1
[0060] Step 1: ultrasonically disperse 10 g of graphene oxide nanoparticles in a 1.5% heptadecafluorodecyltrimethoxysilane solution for 20 min, centrifuge, wash and vacuum dry the ultrasonically dispersed solution for 12 h to obtain hydrophobically modified graphene oxide nanoparticles, wherein the thickness of the graphene oxide nanoparticles is 1-6 nm, the sheet diameter is 1-5 μm, the content of perfluorosilane in the perfluorosilane solution is 1.5 wt %, the content of hydrogen fluoride is 1.5 wt %, the content of ethanol is 85 wt %, and the content of water is 12 wt %.
[0061] Step 2: Grind the hydrophobically modified graphene oxide nanoparticles in 20g of fluoroether oil and ultrasonically disperse them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension, wherein the fluoroether oil is a mixture of CF3CF2CF2O (CF(CF3)CF2O)2CF=CF2 and CF3O(CF2O)4CF=CF2, and the mass ratio of the two is 1:1.5.
[0062] Step 3: emulsion polymerization of 30% of the total mass of hydrophobically modified graphene oxide fluorine ether oil suspension with 100g of copolymerized fluorine-containing monomer and 3g of vulcanization point monomer 3-bromoperfluoro(propyl vinyl) ether, the reaction temperature is 100°C, and then the remaining part of the graphene oxide fluorine ether oil suspension is added dropwise, and the reaction temperature is 120°C to obtain a fluoroelastomer composite emulsion containing modified graphene oxide. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 35wt%, and the rest is 45wt% of vinylidene fluoride and 20wt% of hexafluoropropylene.
[0063] Step 4: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0064] Step 5: Thinly pass, mix, compression mold and perform secondary vulcanization on the fluoroelastomer and 10 g of carbon black filler to obtain a fluoroelastomer composition.
[0065] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 165°C, and compression time 5 min.
[0066] The secondary vulcanization conditions are as follows: vulcanization temperature 200°C, vulcanization time 24 hours.
[0067] Example 2
[0068] Step 1: Ultrasonic dispersion of 5 g of graphene oxide nanoparticles in a 4% heptadecafluorodecyltrimethoxysilane solution for 20 min, centrifugation, washing and vacuum drying of the ultrasonically dispersed solution for 12 h to obtain hydrophobically modified graphene oxide nanoparticles, wherein the thickness of the graphene oxide nanoparticles is 1-6 nm, the sheet diameter is 1-5 μm, the content of perfluorosilane in the perfluorosilane solution is 4 wt %, the content of hydrogen fluoride is 1 wt %, the content of ethanol is 80 wt %, and the content of water is 15 wt %.
[0069] Step 2: Grind the hydrophobically modified graphene oxide nanoparticles in 7 g of fluoroether oil and ultrasonically disperse them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension, wherein the fluoroether oil is a mixture of CF3CF2CF2O(CF(CF3)CF2O)1CF=CF2 and CF3O(CF2O)5CF=CF2, and the mass ratio of the two is 1:1.8.
[0070] Step 3: emulsion polymerization of 20% of the total mass of hydrophobically modified graphene oxide fluoroether oil suspension with 100g of copolymerized fluorinated monomer and 1g of curing point monomer chlorotrifluoroethylene, the reaction temperature is 80°C, and then the remaining part of the graphene oxide fluoroether oil suspension is added dropwise, the reaction temperature is 130°C, and a fluoroelastomer composite emulsion containing modified graphene oxide is obtained. The copolymerized fluorinated monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 60w%, and the rest is 30wt% of vinylidene fluoride and 10wt% of perfluorophenoxypropyl vinyl ether.
[0071] Step 4: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0072] Step 5: Thin-pass, mix, compression-form and secondary-cured the fluoroelastomer and 7 g of carbon nanotube filler to obtain a fluoroelastomer composition.
[0073] The compression molding conditions are as follows: compression pressure 10 MPa, compression temperature 160°C, and compression time 10 min.
[0074] The secondary vulcanization conditions are as follows: vulcanization temperature 210°C, vulcanization time 18 hours.
[0075] Example 3
[0076] Step 1: Ultrasonic dispersion of 15 g of graphene oxide nanoparticles in a 2% perfluorodecyltriethoxysilane solution for 20 min, centrifugation, washing and vacuum drying of the ultrasonically dispersed solution for 12 h to obtain hydrophobically modified graphene oxide nanoparticles, wherein the thickness of the graphene oxide nanoparticles is 1-6 nm, the sheet diameter is 1-5 μm, the content of perfluorosilane in the perfluorosilane solution is 2 wt%, the content of hydrogen fluoride is 1 wt%, the content of ethanol is 85 wt%, and the content of water is 12 wt%.
[0077] Step 2: Grind the hydrophobically modified graphene oxide nanoparticles in 20g of fluoroether oil and ultrasonically disperse them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension, wherein the fluoroether oil is a mixture of CF3CF2CF2O (CF(CF3)CF2O)CF=CF2 and CF3O(CF2O)6CF=CF2, and the mass ratio of the two is 1:2.
[0078] Step 3: emulsion polymerization of 30% of the total mass of hydrophobically modified graphene oxide fluoroether oil suspension with 100g of copolymerized fluorinated monomer and 5g of vulcanization point monomer vinyl chloride, the reaction temperature is 120°C, and then the remaining part of the graphene oxide fluoroether oil suspension is added dropwise, the reaction temperature is 160°C, and a fluoroelastomer composite emulsion containing modified graphene oxide is obtained. The copolymerized fluorinated monomer consists of tetrafluoroethylene, vinylidene fluoride and perfluoroalkyl vinyl ether, wherein the content of tetrafluoroethylene is 45wt%, and the rest is 40wt% of vinylidene fluoride and 15wt% of hexafluoropropylene.
[0079] Step 4: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0080] Step 5: Thinly pass the fluoroelastomer and 10 g of graphene filler, mix, compression mold and perform secondary vulcanization to obtain a fluoroelastomer composition.
[0081] The compression molding conditions are as follows: compression pressure 12 MPa, compression temperature 170°C, and compression time 10 min.
[0082] The secondary vulcanization conditions are as follows: vulcanization temperature 220°C, vulcanization time 24 hours.
[0083] Example 4
[0084] Step 1: Ultrasonic dispersion of 10 g of graphene oxide nanoparticles in a 2% perfluorodecyltriethoxysilane solution for 20 min, centrifugation, washing and vacuum drying of the ultrasonically dispersed solution for 12 h to obtain hydrophobically modified graphene oxide nanoparticles, wherein the thickness of the graphene oxide nanoparticles is 1-6 nm, the sheet diameter is 1-5 μm, the content of perfluorosilane in the perfluorosilane solution is 2 wt%, the content of hydrogen fluoride is 4 wt%, the content of ethanol is 82 wt%, and the content of water is 12 wt%.
[0085] Step 2: Grind the hydrophobically modified graphene oxide nanoparticles in 25g of fluoroether oil and ultrasonically disperse them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension, wherein the fluoroether oil is a mixture of CF3CF2CF2O(CF(CF3)CF2O)3CF=CF2 and CF3O(CF2O)2CF=CF2, and the mass ratio of the two is 1:1.
[0086] Step 3: emulsion polymerization of 10% of the total mass of hydrophobically modified graphene oxide fluoroether oil suspension with 100g of copolymerized fluorine-containing monomer and 5g of vulcanization point monomer isobutylene, the reaction temperature is 80°C, and then the remaining part of the graphene oxide fluoroether oil suspension is added dropwise, the reaction temperature is 110°C, to obtain a fluoroelastomer composite emulsion containing modified graphene oxide, copolymerized fluorine-containing monomer. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 40wt%, and the rest is 35wt% of perfluorophenoxypropyl vinyl ether and 25wt% of perfluoroalkyl vinyl ether.
[0087] Step 4: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0088] Step 5: Thinly pass the fluoroelastomer and 10 g of graphene filler, mix, compression mold and perform secondary vulcanization to obtain a fluoroelastomer composition.
[0089] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0090] The secondary vulcanization conditions are as follows: vulcanization temperature 210°C, vulcanization time 14 hours.
[0091] Comparative Example 1
[0092] 100g of copolymerized fluorine-containing monomer and 4g of 3-bromoperfluoro(propyl vinyl) ether, a vulcanization point monomer, are subjected to emulsion polymerization to obtain a fluoroelastomer emulsion. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 35wt%, and the rest is 45wt% of vinylidene fluoride and 20wt% of hexafluoropropylene.
[0093] The fluoroelastomer composite emulsion is coagulated, washed, dried, and thin-passed to obtain a fluoroelastomer. The fluoroelastomer and 20 g of carbon black filler are thin-passed, mixed, compression-molded, and secondarily vulcanized to obtain a fluoroelastomer composition.
[0094] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0095] The secondary vulcanization conditions are as follows: vulcanization temperature 200°C, vulcanization time 24 hours.
[0096] Comparative Example 2
[0097] 100g of copolymerized fluorine-containing monomer and 4g of 3-bromoperfluoro(propyl vinyl) ether, a vulcanization point monomer, are subjected to emulsion polymerization to obtain a fluoroelastomer emulsion. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 60wt%, and the rest is 30wt% of vinylidene fluoride and 10wt% of perfluorophenoxypropyl vinyl ether.
[0098] The fluoroelastomer composite emulsion is coagulated, washed, dried, and thin-passed to obtain a fluoroelastomer. The fluoroelastomer and 20 g of carbon black filler are thin-passed, mixed, compression-molded, and secondarily vulcanized to obtain a fluoroelastomer composition.
[0099] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0100] The secondary vulcanization conditions are as follows: vulcanization temperature 210°C, vulcanization time 18 hours.
[0101] Comparative Example 3
[0102] 100g of copolymerized fluorine-containing monomer and 3g of curing point monomer chlorotrifluoroethylene are subjected to emulsion polymerization to obtain a fluoroelastomer emulsion. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 35wt%, and the rest is 40wt% of vinylidene fluoride and 25wt% of hexafluoropropylene.
[0103] The fluoroelastomer composite emulsion is coagulated, washed, dried, and thin-passed to obtain a fluoroelastomer. The fluoroelastomer and 25 g of graphene filler are thin-passed, mixed, compression-molded, and secondarily vulcanized to obtain a fluoroelastomer composition.
[0104] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0105] The secondary vulcanization conditions are as follows: vulcanization temperature 220°C, vulcanization time 24 hours.
[0106] Comparative Example 4
[0107] 100g of copolymerized fluorine-containing monomer and 3g of curing point monomer chlorotrifluoroethylene are subjected to emulsion polymerization to obtain a fluoroelastomer emulsion. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 50wt%, and the rest is 35wt% of vinylidene fluoride and 15wt% of perfluorophenoxypropyl vinyl ether.
[0108] The fluoroelastomer composite emulsion is coagulated, washed, dried, and thin-passed to obtain a fluoroelastomer. The fluoroelastomer and 20 g of carbon black filler are thin-passed, mixed, compression-molded, and secondarily vulcanized to obtain a fluoroelastomer composition.
[0109] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0110] The secondary vulcanization conditions are as follows: vulcanization temperature 200°C, vulcanization time 24 hours.
[0111] Comparative Example 5
[0112] Step 1: emulsion polymerize the polyfluorinated monomer and 5g of the vulcanization point monomer isobutylene at a reaction temperature of 80°C, then dropwise add the remaining part of the graphene oxide fluoroether oil suspension at a reaction temperature of 110°C to obtain a fluoroelastomer composite emulsion containing modified graphene oxide, and copolymerize the fluorinated monomer. The copolymerized fluorinated monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 40wt%, and the rest is 35wt% of perfluorophenoxypropyl vinyl ether and 25wt% of perfluoroalkyl vinyl ether.
[0113] Step 2: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0114] Step 3: Thinly pass, mix, compression mold and perform secondary vulcanization on the fluoroelastomer and 11 g of graphene filler to obtain a fluoroelastomer composition.
[0115] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0116] The secondary vulcanization conditions are as follows: vulcanization temperature 210°C, vulcanization time 14 hours.
[0117] Comparative Example 6
[0118] Step 1: Ultrasonic dispersion of 11 g of graphene oxide nanoparticles in a 2% perfluorodecyltriethoxysilane solution for 20 min, centrifugation, washing and vacuum drying of the ultrasonically dispersed solution for 12 h to obtain hydrophobically modified graphene oxide nanoparticles, wherein the thickness of the graphene oxide nanoparticles is 1-6 nm, the sheet diameter is 1-5 μm, the content of perfluorosilane in the perfluorosilane solution is 2 wt%, the content of hydrogen fluoride is 4 wt%, the content of ethanol is 82 wt%, and the content of water is 12 wt%.
[0119] Step 2: Grind the hydrophobically modified graphene oxide nanoparticles in 25g of fluoroether oil and ultrasonically disperse them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension, wherein the fluoroether oil is a mixture of CF3CF2CF2O(CF(CF3)CF2O)3CF=CF2 and CF3O(CF2O)2CF=CF2, and the mass ratio of the two is 1:1.
[0120] Step 3: emulsion polymerization of the hydrophobically modified graphene oxide fluoroether oil suspension with 100g copolymerized fluorine-containing monomer and 5g vulcanization point monomer isobutylene, the reaction temperature is 80°C, and then the remaining part of the graphene oxide fluoroether oil suspension is added dropwise, the reaction temperature is 110°C, to obtain a fluoroelastomer composite emulsion containing modified graphene oxide, copolymerized fluorine-containing monomer. The copolymerized fluorine-containing monomer consists of tetrafluoroethylene, vinylidene fluoride and hexafluoropropylene, wherein the content of tetrafluoroethylene is 40wt%, and the rest is 35wt% of perfluorophenoxypropyl vinyl ether and 25wt% of perfluoroalkyl vinyl ether.
[0121] Step 4: coagulating the fluoroelastomer composite emulsion, washing, drying and thinning to obtain a fluoroelastomer;
[0122] Step 5: directly thin-pass, mix, mold and perform secondary vulcanization on the fluoroelastomer to obtain a fluoroelastomer composition.
[0123] The compression molding conditions are as follows: compression pressure 8 MPa, compression temperature 175°C, and compression time 16 min.
[0124] The secondary vulcanization conditions are as follows: vulcanization temperature 210°C, vulcanization time 14 hours.
[0125] Table 1 Main test results of the examples and comparative examples of this application
[0126]
[0127]
[0128] From the resistivity point of view, antistatic material refers to the resistivity of 10 4 -10 10 Ω·m range of materials, where the resistivity is 104 -10 6 Materials within Ω·m have the best antistatic performance; materials with a resistivity of 10 6 -10 8 Ω·m materials have good anti-static properties; resistivity is 10 8 -10 10 The materials within Ω·m have certain anti-static properties, and anti-static materials are basically semiconductor materials.
[0129] It can be seen from Examples 1-4 that the fluoroelastomer composition prepared from the graphene and fluoroelastomer composite material of the present application has good antistatic and mechanical properties.
[0130] From the experimental results, it can be seen that the hydrophobically modified graphene oxide not only plays the role of nanofiller reinforcement in fluoroelastomer, but also forms a conductive network in the fluoroelastomer matrix to give full play to its conductive effect.
[0131] Conductive carbon black is weaker than graphene in terms of conductivity. However, since graphene is difficult to disperse, adding graphene during thin-ply mixing does not play a good role, as shown in Examples 1-3. Adding graphene oxide during emulsion polymerization plays a key role. For example, 15 g is added in Example 3, which is greater than that in Examples 1 and 2. It is found that Example 3 has the lowest resistivity, which is 5.9×10 4 Ω·m, with the best antistatic performance.
[0132] Compared with Comparative Examples 1-4, graphene can be well dispersed in the fluoroelastomer during emulsion polymerization, and can be antistatic while also improving the mechanical properties of the fluoroelastomer composition.
[0133] By comparing Example 4, Comparative Example 5 and Comparative Example 6, it can be seen that adding the same mass of graphene as that in Example 4 during the emulsion polymerization or thin-pass mixing process cannot achieve the same conductivity as that in Example 4, that is, by adding carbon-containing fillers during the emulsion polymerization and thin-pass mixing processes, a bridging structure is formed between the carbon-containing fillers, which improves the antistatic performance of the fluoroelastomer composition. Compared with adding in a single step, the agglomeration of the carbon-containing filler is reduced, and the antistatic performance of the elastomer is improved.
[0134] In this specification, the same or similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments described later, the description is relatively simple, and the relevant parts can be referred to the partial description of the previous embodiments.
[0135] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing an antistatic fluoroelastomer composition, Features: include S1: placing graphene oxide nanoparticles in a mixed solution of ethanol and water containing perfluorosilane and hydrogen fluoride for ultrasonic dispersion, and separating, washing and drying the solution after ultrasonic dispersion to obtain hydrophobically modified graphene oxide nanoparticles; S2: grinding the hydrophobically modified graphene oxide nanoparticles in fluoroether oil and ultrasonically dispersing them to obtain a hydrophobically modified graphene oxide fluoroether oil suspension; S3: firstly subjecting 10-30% of the total weight of hydrophobically modified graphene oxide fluoroether oil suspension to emulsion polymerization with copolymerized fluorine-containing monomer and vulcanization point monomer, and then adding the remaining part of the graphene oxide fluoroether oil suspension dropwise to obtain a fluoroelastomer composite emulsion containing modified graphene oxide, wherein the graphene oxide nanoparticles are 5-15wt% of the weight of the copolymerized fluorine-containing monomer; S4: washing, drying and thinning the fluoroelastomer composite emulsion after coagulation to obtain a fluoroelastomer; S5: thin-pass, knead, compression-form and secondary-vulcanize the fluoroelastomer to obtain a fluoroelastomer composition, and add a carbon-containing filler during the thin-pass and kneading process, wherein the carbon-containing filler is 5-10wt% of the mass of the copolymerized fluorine-containing monomer.
2. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The copolymerized fluorine-containing monomer is composed of a copolymer formed by tetrafluoroethylene and at least one of the following monomers: vinylidene fluoride, hexafluoropropylene, perfluorophenoxypropyl vinyl ether and perfluoroalkyl vinyl ether.
3. The method for preparing the antistatic fluoroelastomer composition according to claim 2, Features: The content of tetrafluoroethylene in the copolymerized fluorine-containing monomer is 31-60 wt %.
4. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The graphene oxide nanoparticles have a thickness of 1-6 nm and a sheet diameter of 1-5 μm.
5. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The perfluorosilane is heptadecafluorodecyltrimethoxysilane or perfluorodecyltriethoxysilane.
6. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The fluoroether oil is CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)nCF=CF 2 , n = 1-5 and CF 3 O(CF 2 O)mCF=CF 2 , m = 1-6 mixture, the CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)nCF=CF 2 With CF 3 O(CF 2 O)mCF=CF 2 The mass ratio is 1:1-2.
7. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The mass ratio of the hydrophobically modified graphene oxide nanoparticles to the fluoroether oil is 1:1-2.
8. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The vulcanization point monomer is chlorotrifluoroethylene, vinyl chloride, propylene, isobutylene or 3-bromoperfluoro(propyl vinyl) ether, and the amount of the vulcanization point monomer added is 0.5-5wt% of the mass of the copolymerized fluorine-containing monomer.
9. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The carbon-containing filler includes one or more of graphene, carbon nanotubes and carbon black.
10. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: The compression molding conditions are: a compression pressure of 8-12 MPa, a compression temperature of 160-175° C., and a compression time of 5-16 min; the secondary vulcanization conditions are: a vulcanization temperature of 200-220° C., and a vulcanization time of 10-24 hr.
11. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: In S3, the temperature of the emulsion polymerization is 80-120°C, and during the addition of the remaining portion of the graphene oxide fluoroether oil suspension, the reaction temperature increases by 20-50°C.
12. The method for preparing the antistatic fluoroelastomer composition according to claim 1, Features: In S1, the perfluorosilane solution contains 0.5-4wt% perfluorosilane, 0.5-4wt% hydrogen fluoride, 80-85wt% ethanol, and the rest is water.