Ionic gel as well as preparation method and application thereof

By introducing zirconium oxychloride into ionic gels to form complexation, the lack of performance of existing ionic gels under high strain and high strength conditions has been solved, and the conductive and mechanical properties have been improved. It is suitable for wearable devices , gel electrode sheet and strain sensor applications.

CN119080991AActive Publication Date: 2024-12-06NAT UNIV OF DEFENSE TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411265847.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Existing ionic gels exhibit low conductivity, low fracture strength and poor fracture toughness under large strain, cyclic stress and high strength conditions, which limits their application scenarios.

Method used

By introducing zirconium oxychloride into the polymer, physical crosslinking is achieved and conductive and mechanical properties are improved by using the four positive charges of zirconium ions and the multi-dentate ligand properties of sulfonic acid groups.

Benefits of technology

The simultaneous improvement of the conductivity and mechanical properties of the ion gel is achieved, the fracture strength can reach 2.98MPa, the fracture strain rate reaches 575%, and excellent environmental stability and low temperature resistance are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080991A_ABST
    Figure CN119080991A_ABST
Patent Text Reader

Abstract

The invention discloses ionic gel as well as a preparation method and application thereof, and belongs to the technical field of ionic gel. The preparation method of the ionic gel comprises the following steps: S1, adding a photoinitiator and a zirconium oxychloride solution with a certain concentration into a mixed solution of a polymer monomer and an ionic liquid, and heating and stirring until the mixture is completely dissolved; s2, dispersing and defoaming the solution obtained in the step S1 to obtain a precursor solution; and S3, carrying out polymerization reaction on the precursor solution obtained in S2 under the irradiation of ultraviolet light to obtain the metal complex ion gel. The metal complex ion gel provided by the invention has excellent mechanical properties, conductivity, environmental stability and low temperature resistance, keeps high adhesion performance on the surfaces of materials such as polyvinyl chloride, copper, glass and stainless steel, and can be applied to devices such as wearable equipment, gel electrode plates, soft robots and strain sensors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ion gel, and in particular relates to an ion gel and a preparation method and application thereof. Background Art

[0002] Ion gel is a gel-like flexible material composed of high molecular organic polymers and salt electrolytes (ionic liquids) that can be electrolyzed into ions. Ion gel has high ionic conductivity, electrochemical stability and good deformation ability. But in fact, although in theory ion gel can meet the requirements of good electrical conductivity and mechanical properties at the same time, most of the current ion gels have the disadvantages of low conductivity, low fracture strength and poor fracture toughness, which cannot meet the use of ion gels under large strain, cyclic stress and high strength conditions, thus greatly limiting the application scenarios of ion gels. Summary of the invention

[0003] The problem to be solved by the present invention is to provide an ion gel and a preparation method and application thereof, and to improve the strength and conductivity of the ion gel through metal complexation, thereby solving the problem that the ion gel in the prior art cannot obtain high mechanical properties and conductive properties.

[0004] The present invention includes a method for preparing an ion gel, comprising the following steps:

[0005] S1, adding a photoinitiator and a certain concentration of zirconium oxychloride solution to a mixed solution of polymer monomers and ionic liquids, heating and stirring until completely dissolved;

[0006] S2, dispersing and defoaming the solution obtained in S1 to obtain a precursor solution;

[0007] S3, subjecting the precursor solution obtained in S2 to polymerization reaction under ultraviolet light to obtain a metal complex ion gel.

[0008] Furthermore, in S1, the molar concentration of the zirconium oxychloride solution is 0.5 mol / L-0.875 mol / L.

[0009] Furthermore, in S1, the polymer monomers include acrylic acid and 2-acrylamido-2-methyl-1-propane sulfonic acid, and the ratio of acrylic acid to 2-acrylamido-2-methyl-1-propane sulfonic acid is 9:1.

[0010] Furthermore, in S1, the ionic liquid includes 1-ethyl-3-methylimidazolium acetate.

[0011] Furthermore, in S1, the photoinitiator includes 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, and the molar percentage of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone to the polymer monomer is 1%.

[0012] Furthermore, in S1, the heating temperature during heating and stirring is 80°C-90°C, the stirring rate is 300rpm-600rpm, and the time is 0.3h-1h.

[0013] Furthermore, in S2, the solution obtained in S1 is placed in an ultrasonic cleaning machine for dispersion and bubbling; the cleaning power of the ultrasonic cleaning machine is 300W, and the cleaning time is 15min-30min.

[0014] Furthermore, in S3, the precursor solution obtained in S2 is placed in an ultraviolet light machine for polymerization reaction; the working wavelength of the ultraviolet light machine is 365nm, and the working power is 100W; the polymerization reaction time is 10min-20min.

[0015] As a general inventive concept, the present invention also provides an ion gel, which is prepared by the above-mentioned method for preparing the ion gel.

[0016] As a general inventive concept, the present invention also provides an application of an ion gel, wherein the ion gel is applied to a wearable device, a gel electrode sheet, a soft robot or a strain sensor.

[0017] Beneficial effects of the present invention:

[0018] The preparation method of the ion gel provided by the present invention forms a stable complex by introducing zirconium oxychloride into the polymer. Compared with other low-valent metal ions such as aluminum ions and iron ions, on the one hand, zirconium ions carry four positive charges and have a smaller radius, and have a good ability to accept non-bonding electron pairs. On the other hand, the sulfonic acid group is a hard base and can be used as a multi-dentate ligand to coordinate with the zirconium ion. Its coordination ability is stronger than that of the monodentate ligand. Therefore, the complex ligand formed by zirconium oxychloride is usually more stable than the individual ligands or central ions composed of it, thereby playing a role of physical cross-linking between polymer molecular chains. The complex ligand formed based on zirconium oxychloride can transfer electrons through the charge from the metal to the ligand. These characteristics effectively improve the electrical conductivity and mechanical properties of the ionic liquid; in addition, the ionic liquid can provide a conductive path as a dispersed phase in the gel, and the ionic liquid has different solubility with the two-phase polymer. The structure of the combination of the soft phase and the hard phase can effectively improve the strength and toughness of the ion gel, thereby achieving the simultaneous improvement of mechanical properties and electrical conductivity.

[0019] The metal complexation-based ion gel preparation method provided by the present invention can adjust the mechanical and electrical properties of the ion gel by regulating the metal ion content in the system. Experiments show that through component regulation, the fracture strength of the ion gel can reach up to 2.98MPa while maintaining a fracture strain of 575%.

[0020] The metal complex ion gel provided by the invention has excellent environmental stability and low temperature resistance, and maintains relatively high adhesion performance on the surfaces of materials such as polyvinyl chloride, copper, glass and stainless steel.

[0021] The metal complex ion gel provided by the present invention can be applied to devices such as wearable devices, gel electrode sheets, soft robots and strain sensors. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Attached Figure 1 is a process flow chart of the method for preparing the ion gel of the present invention;

[0023] Attached Figure 2 The infrared spectra of ion gels at different zirconium oxychloride contents, where (a) is 4000~400cm -1 Infrared spectra in the wavenumber range, (b) 1200~700cm -1 Infrared spectra in a range of wavenumbers;

[0024] Attached Figure 3 is the conductivity of ion gel at different zirconium oxychloride contents;

[0025] Attached Figure 4 1 is a stress-strain curve diagram of the ion gel in Examples 1-3 and Comparative Example 2;

[0026] Attached Figure 5 The variable strain cyclic stretching diagram of the ion gel of Example 3 and the energy dissipation of the ion gel under different tensile strain conditions, wherein (a) is the variable strain cyclic stretching diagram of the ion gel, and (b) is the energy dissipation of the ion gel under different tensile strain conditions;

[0027] Attached Figure 6 is a differential scanning calorimetry analysis diagram of the ion gel of Example 3;

[0028] Attached Figure 7 This is the thermogravimetric analysis diagram of the ion gel of Example 3;

[0029] Attached Figure 8 Schematic diagrams of four surface adhesion properties of the ion gel of Example 3, wherein (a) is a schematic diagram of the ion gel adhesion performance test, and (b) is a diagram of the adhesion test results of the ion gel on different surfaces;

[0030] Attached Fig. 9 The dissolution conditions of the solutions at different heating and stirring temperatures in Comparative Example 2 and Example 1 are shown;

[0031] Attached Fig.10 This is the stress-strain curve when the zirconium oxychloride concentration in Comparative Example 3 is 0.25 mol / L. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not intended to limit the present invention.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0034] Unless otherwise specified, all drugs / reagents used were commercially available.

[0035] As attached Figure 1 As shown, an embodiment of the present invention provides a method for preparing an ion gel, comprising the following steps:

[0036] S1, adding a photoinitiator and a certain concentration of zirconium oxychloride solution to a mixed solution of polymer monomers and ionic liquids, heating and stirring until completely dissolved;

[0037] S2, dispersing and defoaming the solution obtained in S1 to obtain a precursor solution;

[0038] S3, subjecting the precursor solution obtained in S2 to polymerization reaction under ultraviolet light to obtain a metal complex ion gel.

[0039] The preparation method of the ion gel provided by the embodiment of the present invention forms a stable complex by introducing zirconium oxychloride into the polymer. Compared with other low-valent metal ions such as aluminum ions and iron ions, on the one hand, zirconium ions carry four positive charges and have a small radius, and have a good ability to accept non-bonding electron pairs. On the other hand, the sulfonic acid group is a hard base and can be used as a multi-dentate ligand to coordinate with the zirconium ion. Its coordination ability is stronger than that of the monodentate ligand. Therefore, the complex ligand formed by zirconium oxychloride is usually more stable than the individual ligands or central ions it constitutes, thereby playing a role of physical cross-linking between polymer molecular chains. The complex ligand formed based on zirconium oxychloride can transfer electrons through the charge from the metal to the ligand. These characteristics effectively improve the conductivity and mechanical properties of the ionic liquid; in addition, the ionic liquid can provide a conductive path as a dispersed phase in the gel, and the ionic liquid has different solubility with the two-phase polymer. The structure of the combination of the soft phase and the hard phase can effectively improve the strength and toughness of the ion gel, thereby achieving the simultaneous improvement of mechanical properties and conductive properties.

[0040] The metal complexation-based ion gel preparation method provided in the embodiment of the present invention can adjust the mechanical and electrical properties of the ion gel by adjusting the ratio of the two-phase polymers and the metal ion content in the system. Experiments show that by adjusting the components, the fracture strength of the ion gel can reach up to 2.98MPa while maintaining a fracture strain of 575%.

[0041] In a preferred embodiment, in S1, the molar concentration of the zirconium oxychloride solution is 0.5mol / L-0.875mol / L; the concentration of zirconium oxychloride is different, and the content of the introduced metal ions is different. The ion gel preparation method provided by the present invention can adjust the mechanical properties and electrical conductivity of the ion gel by regulating the content of metal ions. The higher the molar concentration of the introduced zirconium oxychloride, the better the conductivity of the obtained ion gel. Within the preferred range of this embodiment, the ion gel can simultaneously obtain higher mechanical properties. Within this range, the ion gel has both excellent mechanical properties and electrical conductivity. More preferably, the molar concentration of the zirconium oxychloride solution is 0.5mol / L-0.75mol / L. Most preferably, the molar concentration of the zirconium oxychloride solution is 0.75mol / L, at which time the obtained ion gel has excellent conductivity and the best mechanical properties.

[0042] In a preferred embodiment, in S1, the polymer monomers include acrylic acid (PAA) and 2-acrylamido-2-methyl-1-propane sulfonic acid (PAMPS), and the ratio of acrylic acid to 2-acrylamido-2-methyl-1-propane sulfonic acid is 9:1.

[0043] In a preferred embodiment, in S1, the ionic liquid includes 1-ethyl-3-methylimidazolium acetate, and the added amount thereof is calculated by converting the ratio of different polymer systems into volume.

[0044] In a preferred embodiment, in S1, the molar percentage of the photoinitiator to the polymer monomer is 1%; the high content of the photoinitiator reduces the inhibitory effect of oxygen in the air on the polymerization reaction during the photoinitiation process, ensuring that the monomer is fully polymerized. Optionally, the photoinitiator includes 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0045] In a preferred embodiment, in S1, the heating temperature during heating and stirring is 80°C-90°C, the stirring rate is 300rpm-600rpm, and the time is 0.3h-1h; more preferably, the stirring rate is 500rpm, and the time is 0.3h; when the temperature is lower than 80°C, zirconium oxychloride and the initiator cannot be fully dissolved in the ionic liquid, and too high a temperature will cause thermal initiation of the initiator, thereby causing the polymerization reaction to occur prematurely.

[0046] In a preferred embodiment, in S2, the solution obtained in S1 is placed in an ultrasonic cleaning machine for dispersion and bubbling; the cleaning power of the ultrasonic cleaning machine is 300W, and the cleaning time is 15min-30min; ultrasound makes the solution disperse more evenly and effectively removes the air mixed in the solution due to stirring. If the ultrasonic time is too short, the air cannot be fully removed, and if the ultrasonic time is too long, the solution temperature will rise and cause the polymer to cross-link.

[0047] In a preferred embodiment, in S3, the precursor solution obtained in S2 is placed in an ultraviolet light machine for polymerization reaction; the working wavelength of the ultraviolet light machine is 365nm, and the working power is 100W; the polymerization reaction time is 10min-20min; as the zirconium oxychloride content increases, the time required for initiation gradually increases, and when the reaction time is too short, the crosslinking is incomplete and no gel can be formed.

[0048] An embodiment of the present invention also provides an ion gel, which is prepared by any of the above-mentioned methods for preparing ion gels; the ion gel includes a dispersed phase composed of an ionic liquid and a polymer phase composed of a two-phase polymer, the ionic liquid has a high bulk conductivity, and as a dispersed phase, it can also provide a conductive path, thereby improving the electrical properties of the gel, the two-phase polymer has different compatibilities in the ionic liquid, and thus exhibits mechanical properties with both strength and toughness, and by introducing metal ions into the polymer, the conductive properties and mechanical properties of the ionic liquid are further improved through metal complexation; the metal complex ion gel provided by the embodiment of the present invention has excellent environmental stability and low temperature resistance, and maintains high adhesion properties on the surfaces of materials such as polyvinyl chloride, copper, glass and stainless steel.

[0049] An embodiment of the present invention also provides an application of an ion gel, wherein the metal complex ion gel provided by the present invention is applied to a wearable device, a gel electrode sheet, a soft robot or a strain sensor.

[0050] Example 1

[0051] This embodiment provides a method for preparing an ion gel, comprising the following steps:

[0052] S1. Add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator) to a mixed solution of 2-acrylamido-2-methyl-1-propane sulfonic acid and polyacrylic acid monomers in a molar ratio of 1:9, and then add zirconium oxychloride with a molar concentration of 0.50 mol / L, and finally add 2.35 ml of 1-ethyl-3-methylimidazolium acetate (ionic liquid) to make a 10 ml solution, and then place it on a heated magnetic stirrer and heat and stir until it is completely dissolved, the heating temperature is 90° C., the heating time is 30 min, and the stirring rate is 500 rpm;

[0053] S2, placing the solution after S1 is dissolved in an ultrasonic cleaning machine for dispersion and defoaming, setting the power to 100 W and the time to 20 min to prepare a precursor solution;

[0054] S3. Transfer the precursor solution obtained in S2 into a mold and put it into a UV light machine, set the power to 100 W, and perform polymerization reaction under UV light for 15 minutes to obtain a metal complex ion gel.

[0055] The metal complex ion gel obtained in this example was tested, and the breaking strength reached 0.873MPa, the breaking elongation was 957%, and the breaking energy was 3.37MJ / m 3 , the conductivity is 2.53S / m.

[0056] Example 2

[0057] This embodiment provides a method for preparing an ion gel, comprising the following steps:

[0058] S1. Add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator) to a mixed solution of 2-acrylamido-2-methyl-1-propane sulfonic acid and polyacrylic acid monomers in a molar ratio of 1:9, and then add zirconium oxychloride with a molar concentration of 0.625 mol / L, and finally add 2.04 ml of 1-ethyl-3-methylimidazolium acetate (ionic liquid) to make a 10 ml solution, and then place it on a heated magnetic stirrer and heat and stir until it is completely dissolved, the heating temperature is 90° C., the heating time is 30 min, and the stirring rate is 500 rpm;

[0059] S2, placing the solution after S1 is dissolved in an ultrasonic cleaning machine for dispersion and defoaming, setting the power to 100 W and the time to 20 min to prepare a precursor solution;

[0060] S3. Transfer the precursor solution obtained in S2 into a mold and put it into a UV light machine, set the power to 100 W, and perform polymerization reaction under UV light for 15 minutes to obtain a metal complex ion gel.

[0061] The metal complex ion gel obtained in this example was tested, and the breaking strength reached 2.00 MPa, the breaking elongation was 886%, and the breaking energy was 7.76 MJ / m 3 , the conductivity is 4.23S / m.

[0062] Example 3

[0063] This embodiment provides a method for preparing an ion gel, comprising the following steps:

[0064] S1. Add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator) to a mixed solution of 2-acrylamido-2-methyl-1-propane sulfonic acid and polyacrylic acid monomers in a molar ratio of 1:9, and then add zirconium oxychloride with a molar concentration of 0.75 mol / L, and finally add 2.30 ml of 1-ethyl-3-methylimidazolium acetate (ionic liquid) to make a 10 ml solution, and then place it on a heated magnetic stirrer and heat and stir until it is completely dissolved, the heating temperature is 90° C., the heating time is 30 min, and the stirring rate is 500 rpm;

[0065] S2, placing the solution after S1 is dissolved in an ultrasonic cleaning machine for dispersion and defoaming, setting the power to 100 W and the time to 20 min to prepare a precursor solution;

[0066] S3. Transfer the precursor solution obtained in S2 into a mold and put it into a UV light machine, set the power to 100 W, and perform polymerization reaction under UV light for 15 minutes to obtain a metal complex ion gel.

[0067] The metal complex ion gel obtained in this example was tested, and the breaking strength reached 2.98 MPa, the breaking elongation was 575%, and the breaking energy was 7.76 MJ / m 3 , the conductivity is 6.69S / m.

[0068] The performance of the ion gel samples prepared by introducing different concentrations of zirconium oxychloride was tested. The samples were recorded as PAMPS-co-PAA-1 to PAMPS-co-PAA-8 according to the concentration of zirconium oxychloride from low to high, where the zirconium oxychloride concentration corresponding to each sample is shown in Table 1.

[0069] Table 1 Zirconium oxychloride concentration corresponding to each sample

[0070] Sample Zirconium oxychloride concentration (mol / L) PAMPS-co-PAA-1 0 PAMPS-co-PAA-2 0.125 PAMPS-co-PAA-3 (Comparative Example 3) 0.25 PAMPS-co-PAA-4 0.375 PAMPS-co-PAA-5 (Example 1) 0.5 PAMPS-co-PAA-6 (Example 2) 0.625 PAMPS-co-PAA-7 (Example 3) 0.75 PAMPS-co-PAA-8 0.875

[0071] As shown in Table 1, PAMPS-co-PAA-1 to PAMPS-co-PAA-4 are all lower than the preferred zirconium oxychloride concentration range of 0.5 mol / L-0.875 mol / L of the present invention, PAMPS-co-PAA-3 corresponds to the ion gel prepared in Example 3, PAMPS-co-PAA-5 corresponds to the ion gel prepared in Example 1, PAMPS-co-PAA-6 corresponds to the ion gel prepared in Example 2, and PAMPS-co-PAA-7 corresponds to the ion gel prepared in Example 3.

[0072] As attached Figure 2 As shown in Figure 2, the functional group changes of zirconium oxychloride with different molar concentrations were analyzed by infrared spectrometer. It can be seen from the spectrum that with the continuous increase of zirconium oxychloride content, the signal peak representing the sulfur-oxygen bond (1150cm -1 and 998cm -1 ) underwent a blue shift, indicating that a complex coordination bond was formed between the zirconium ion and the sulfonate.

[0073] As attached Figure 3 As shown, the zirconium oxychloride content of PAMPS-co-PAA-5 to PAMPS-co-PAA-8 increases continuously, and with the continuous increase of zirconium oxychloride content, the conductivity of the ion gel increases continuously. This is mainly because the metal ions improve the ability of electron transfer in the ion gel system, thereby increasing the conductivity of the system and showing a higher conductivity. In Example 3 (PAMPS-co-PAA-67), when the zirconium oxychloride concentration is 0.75 mol / L, the conductivity can reach 6.69 S / m.

[0074] As attached Figure 4 As shown in the figure, the stress-strain curves of the ion gels obtained by introducing a cross-linking agent and different concentrations of zirconium oxychloride, and the stress-strain curves of the ion gels obtained by introducing 0.75 mol / L zirconium oxychloride in Example 3 (PAMPS-co-PAA-7) show that the introduced high-valent metal salt zirconium oxychloride forms a metal complex and exhibits excellent mechanical properties. On the basis of a fracture strength of 2.98 MPa, it can also maintain a fracture strain of 575%, and its fracture energy is 7.76 MJ / m 3 In addition, the conductivity test shows that its conductivity is also at a relatively high level, reaching 6.69S / m.

[0075] As attached Figure 5 As shown, the energy dissipation of the ion gel of Example 3 (PAMPS-co-PAA-7) under different tensile strain conditions, with the increase of strain, the hysteresis loop area gradually increases, indicating that under higher strain conditions, the metal complex ion gel also has excellent energy dissipation performance, so that the ion gel has excellent fracture strength.

[0076] The ion gel of Example 3 (PAMPS-co-PAA-7) was subjected to differential scanning calorimetry and thermogravimetric analysis. Figure 6 As shown in the figure, the results show that in the temperature range of -50°C to 25°C, the heat flow curve of the metal complex ion gel in Example 3 (PAMPS-co-PAA-7) does not show a glass transition, which indicates that in the temperature range of -50°C to 25°C, the ion gel can still maintain good elasticity; as shown in the attached Figure 7 As shown, thermogravimetric analysis shows that the ion gel undergoes significant thermal weight loss above 300°C, indicating that the ion gel has good stability under room temperature to medium and low temperature conditions.

[0077] The ion gel used in the device also requires good adhesion to the substrate to ensure stable signal transmission. Figure 8 As shown, the adhesion strength of the metal complex ion gel prepared in Example 3 (PAMPS-co-PAA-7) on the surfaces of four common materials (plastic, stainless steel, copper, and glass) was tested by shear experiments. Based on the rich hydrogen bonding effect of the ion gel, the ion gel of the embodiment of the present invention showed good bonding properties on the above four surfaces.

[0078] Comparative Example 1

[0079] In this comparative example, crosslinking is performed by adding a crosslinking agent to the polymer system, and other settings are the same as those in Example 1.

[0080] The specific steps include:

[0081] S1. Add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator) at 0.05% of the polymer monomer to a solution of 2-acrylamido-2-methyl-1-propane sulfonic acid and polyacrylic acid monomers in a molar ratio of 1:9, then add N,N-methylenebisacrylamide (cross-linker) at 0.1% of the polymer monomer, and finally add 2.35 ml of 1-ethyl-3-methylimidazolium acetate (ionic liquid) to make a 10 ml solution, then place it on a heated magnetic stirrer and heat and stir until it is completely dissolved, the heating temperature is 90° C., the heating time is 30 min, and the stirring rate is 500 rpm;

[0082] S2, the same as in Example 1;

[0083] S3. Same as Example 1.

[0084] The ion gel of this comparative example was tested, and the breaking strength was 1.06MPa, the breaking elongation was 216%, and the breaking energy was 1.12MJ / m 3 , combined with the attached Figure 4 Compared with Example 1 (PAMPS-co-PAA-5), the ionic gel with the addition of a crosslinker in Comparative Example 1 has a significant decrease in the elongation at break. This is because the addition of the crosslinker forms irreversible chemical bonds in the system, which easily leads to local stress concentration during the stretching process and overall failure of the gel.

[0085] Comparative Example 2

[0086] The heating and stirring temperature in S1 of this comparative example is 60° C., and other settings are the same as those in Example 1.

[0087] As attached Fig. 9 As shown, the left side is the effect after stirring at 60°C for 20 minutes in Comparative Example 2, and the solution is an opaque turbid liquid, indicating that the solute cannot be completely dissolved at this temperature, while the right side is the state after stirring at 90°C for 20 minutes in Example 1, and the liquid is transparent as a whole, indicating that the solute has been completely dissolved.

[0088] Comparative Example 3

[0089] In this comparative example, the amount of zirconium oxychloride added to S1 is 0.25 mol / L, and other settings are the same as those in Example 1.

[0090] The specific steps include:

[0091] S1. Add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator) at 0.05% of the polymer monomer to a mixed solution of 2-acrylamido-2-methyl-1-propane sulfonic acid and polyacrylic acid monomers in a molar ratio of 1:9, then add zirconium oxychloride with a molar concentration of 0.25 mol / L, and finally add 3.04 ml of 1-ethyl-3-methylimidazolium acetate (ionic liquid) to make a 10 ml solution, then place it on a heated magnetic stirrer and heat and stir until it is completely dissolved, the heating temperature is 90° C., the heating time is 30 min, and the stirring rate is 500 rpm;

[0092] S2, the same as in Example 1;

[0093] S3. Same as Example 1.

[0094] The ion gel of this comparative example was tested. Fig.10 As shown, the breaking strength is 0.217MPa, the breaking elongation is 1410%, and the breaking energy is 1.21MJ / m 3 , it can be seen that at lower zirconium oxychloride addition, the ion gel exhibits soft and weak mechanical properties, i.e., higher elongation at break and lower fracture strength.

[0095] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0096] The above-mentioned embodiments only express several implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.

[0097] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.

Claims

1. A method for preparing an ion gel, characterized in that: The following steps are involved: S1, adding a photoinitiator and a certain concentration of zirconium oxychloride solution to a mixed solution of polymer monomers and ionic liquids, heating and stirring until completely dissolved; S2, dispersing and defoaming the solution obtained in S1 to obtain a precursor solution; S3, subjecting the precursor solution obtained in S2 to polymerization reaction under ultraviolet light to obtain a metal complex ion gel.

2. The method for preparing the ion gel according to claim 1, characterized in that: In S1, the molar concentration of the zirconium oxychloride solution is 0.5 mol / L-0.875 mol / L.

3. The method for preparing the ion gel according to claim 1, characterized in that: In S1, the polymer monomers include acrylic acid and 2-acrylamido-2-methyl-1-propane sulfonic acid, and the ratio of acrylic acid to 2-acrylamido-2-methyl-1-propane sulfonic acid is 9:

1.

4. The method for preparing the ion gel according to claim 1, characterized in that: In S1, the ionic liquid includes 1-ethyl-3-methylimidazolium acetate.

5. The method for preparing the ion gel according to claim 1, characterized in that: In S1, the photoinitiator includes 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, and the molar percentage of 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone to the polymer monomer is 1%.

6. The method for preparing the ion gel according to claim 1, characterized in that: In the step S1, the heating temperature during the heating and stirring is 80°C-90°C, the stirring rate is 300rpm-600rpm, and the time is 0.3h-1h.

7. The method for preparing the ion gel according to claim 1, characterized in that: In S2, the solution obtained in S1 is placed in an ultrasonic cleaning machine for dispersion and bubbling; the cleaning power of the ultrasonic cleaning machine is 300W, and the cleaning time is 15min-30min.

8. The method for preparing the ion gel according to claim 1, characterized in that: In S3, the precursor solution obtained in S2 is placed in an ultraviolet light machine to carry out the polymerization reaction; the working wavelength of the ultraviolet light machine is 365nm, and the working power is 100W; the time of the polymerization reaction is 10min-20min.

9. An ion gel, characterized in that: The ion gel is prepared by the preparation method of any one of claims 1 to 8.

10. An application of an ion gel, characterized in that: The ion gel as claimed in claim 9 is applied to wearable devices, gel electrode sheets, soft robots or strain sensors.

Citation Information

Patent Citations

  • Ionic liquid gel electrolyte, preparation method thereof, and application thereof

    CN110148781A

  • Underwater high-strength ionic gel as well as preparation method and application thereof

    CN115232242A

  • Conductive multifunctional gel sensor as well as preparation method and application thereof

    CN116041607A

  • Super-tensile ionic gel as well as preparation method and application thereof

    CN116444739A

  • Super-tough plastic hydrogel and preparation method thereof

    CN117069884A