SiO2 polymer microsphere, preparation method and application thereof, and oil-based drilling fluid

By modifying SiO2 under acidic conditions and polymerizing with water-soluble monomers, amphiphilic SiO2 polymer microspheres were prepared, which solved the problem of insufficient pressure bearing capacity of oil-based drilling fluid leakage plugging materials and improved the leakage plugging success rate And maintain the rheological performance of oil-based drilling fluid.

CN119081027AInactive Publication Date: 2024-12-06SOUTHWEST PETROLEUM UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411381759.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing oil-based drilling fluid leak-proof material has weak pressure bearing capacity, resulting in a low success rate of leakage plugging. The existing research is mainly based on the improvement of water-based drilling fluid, resulting in poor compatibility with oil-based drilling fluid and leak-proof effect. Not good.

Method used

Using SiO2 polymer microsphere material, by modifying SiO2 under acidic conditions and performing reverse suspension polymerization with water-soluble monomers, a macromolecular structure with amphiphilicity, good dispersion and adaptability was prepared for improvement. Leakage plugging performance of oil-based drilling fluid.

Benefits of technology

The good dispersion and leakage plugging performance of SiO2 polymer microspheres in oil-based drilling fluid is achieved, which can effectively plug formation cracks and improve the success rate of leakage plugging at one time, and does not affect the rheology performance of crude oil-based drilling fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070072250000161
    Figure BDA0005070072250000161
  • Figure BDA0005070072250000171
    Figure BDA0005070072250000171
  • Figure BDA0005070072250000172
    Figure BDA0005070072250000172
Patent Text Reader

Abstract

The invention belongs to the field of oilfield chemistry, and discloses an S O2 polymer microsphere, a preparation method and application thereof and an oil-based drilling fluid, and the preparation method of the S O2 polymer microsphere material comprises the following steps: (1) contacting S O2 with a silane coupling agent under an acidic condition for modification to obtain modified S O2; and (2) contacting the modified S < 2 > with three water-soluble monomers, and carrying out free radical polymerization reaction to obtain the S < 2 > polymer microsphere material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plugging materials, and in particular to an oil-based drilling fluid plugging material and a preparation method thereof. Background Art

[0002] With the rapid economic development, the global crude oil resources are almost exhausted in the continuous exploitation. Oil extraction has entered the stage of complex wells and ultra-deep well drilling. Therefore, drilling fluids face the challenges of ultra-high temperature and ultra-high pressure in deep formations. Not only that, with the damage to the reservoir caused by the previous drilling operations, the heterogeneity and surface hydration problems of the reservoir have been further aggravated. Water-based drilling fluids can no longer meet the drilling requirements. Therefore, oil-based drilling fluids have become the first choice due to their excellent lubricity, temperature resistance and inhibition. However, the problem of wellbore instability of oil-based drilling fluids has not been well solved. The drilling fluid invades the formation under the pressure difference, resulting in the development of nano-micron-level cracks in the formation. The collapse pressure increases under the continuous invasion of the drilling fluid, which eventually leads to well leakage.

[0003] At present, the phenomenon of well leakage during drilling operations is very common. According to statistics, the probability of well leakage in 75% of wells using oil-based drilling fluid for production during deep well operations is as high as 80%, and the success rate of one-time plugging is very low. This is mainly due to the lack of plugging materials compatible with oil-based drilling fluids for plugging. The plugging methods are mostly to increase the density of drilling fluids and use rigid particles as plugging agents. These methods can only achieve temporary plugging. Once the formation pressure changes, secondary leakage is likely to occur, resulting in higher resource losses. Compared with these methods, using plugging agents and using their chemical properties to react chemically with the leakage wall to improve the plugging success rate has become an effective method. Nowadays, the research on water-based drilling fluid plugging materials is very mature, while the research on oil-based drilling fluid plugging materials is still in the development stage. Most of the research on oil-based drilling fluid plugging is based on water-based drilling fluid plugging agents and improves them. This leads to poor compatibility of the developed plugging agents with oil-based drilling fluids, resulting in poor plugging effects.

[0004] SiO2, as a multifunctional inorganic material, has attracted attention for many years. However, due to its rich silicon hydroxyl groups on the surface and large surface energy, it will cause it to agglomerate. Therefore, researchers have modified it to improve its dispersibility, but simply modifying it cannot play a good role in its plugging performance. Therefore, combining the physical properties of SiO2 such as temperature resistance and rigidity with the elasticity and water / oil absorption and swelling properties of polymers can open up a new path for plugging leaks in oil-based drilling fluids.

[0005] Therefore, providing a plugging material in an oil-based drilling fluid having good lipophilicity and strong pressure bearing capacity is of great significance for plugging the leakage of the oil-based drilling fluid. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of weak pressure bearing capacity and low one-time plugging success rate of existing oil-based drilling fluid plugging materials, and to provide a preparation method of SiO2 polymer microsphere material and its application as well as oil-based drilling fluid.

[0007] In order to achieve the above object, the first aspect of the present invention provides a method for preparing SiO2 polymer microsphere material, the method comprising:

[0008] (1) SiO2 is contacted with a silane coupling agent under acidic conditions for modification to obtain modified SiO2.

[0009] (2) Modified SiO2 and three water-soluble monomers were polymerized by reverse suspension polymerization to obtain modified

[0010] SiO2 polymer microsphere material.

[0011] The second aspect of the present invention provides a SiO2 polymer microsphere material prepared by the method described in the first aspect.

[0012] The third aspect of the present invention provides the use of the SiO2 polymer microsphere material described in the second aspect as a plugging agent in oil-based drilling fluid.

[0013] The fourth aspect of the present invention provides an oil-based drilling fluid, which contains the SiO2 polymer microsphere material described in the second aspect.

[0014] Through the above technical solution, the present invention can achieve the following beneficial effects:

[0015] (1) The SiO2 polymer microsphere material prepared by the method provided by the present invention has a particle size range of 98-130 μm. The SiO2 polymer microsphere material is amphiphilic, has good dispersibility in both oil and water environments, has good compatibility with oil-based drilling fluid, and has both rigidity and viscoelasticity after absorbing water. This property can improve the plugging performance of the oil-based drilling fluid and effectively plug cracks of corresponding pore sizes.

[0016] (2) The oil-based drilling fluid provided by the present invention contains the aforementioned SiO2 polymer microsphere material, and the addition of the SiO2 polymer microsphere material will not cause a significant impact on the rheological properties of the crude oil-based drilling fluid. Due to its good adaptability and plugging performance, it lays a certain foundation for its on-site application. DETAILED DESCRIPTION

[0017] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise range thresholds, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0019] The first aspect of the present invention provides a method for preparing a SiO2 polymer microsphere material, the method comprising:

[0020] (1) SiO2 is contacted with a silane coupling agent under acidic conditions for modification to obtain modified SiO2.

[0021] According to the present invention, in step (1), the SiO2 is ordinary unmodified SiO2, and there are a large number of unsaturated residual bonds and hydroxyl groups in different bonding states on the surface of SiO2. Because its surface lacks oxygen, it deviates from the stable silicon-oxygen structure and has high reactivity. Therefore, it can be brought into contact with a silane coupling agent under acidic conditions to modify it so that one end of the silane coupling agent is connected to SiO2, and the other end utilizes the C=C double bond of the silane coupling agent to polymerize with other compounds under the action of an initiator and a crosslinking agent to obtain SiO2 polymer microspheres.

[0022] According to the present invention, the SiO2 is spherical SiO2 powder. Specifically, the spherical SiO2 powder has an average particle size of 20 nm, a specific surface area of ​​240 m2 / g, and a purity greater than 99%.

[0023] According to the present invention, the conductivity of the deionized water is ≤0.056 us / cm (25° C.), and the maximum number of bacteria is 0.01 / mL.

[0024] According to the present invention, the pH regulator for creating the acidic condition is selected as a dilute hydrochloric acid standard solution. Specifically, the concentration of the dilute hydrochloric acid standard solution is 0.1000 mol / L and the purity is greater than 99%.

[0025] According to the present invention, preferably, the silane coupling agent is selected from one of vinyl tri(b-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, and methacryloxypropyl trimethoxysilane, and more preferably γ-methacryloxypropyl trimethoxysilane.

[0026] According to the present invention, in step (1), the weight ratio of the ethanol solution to deionized water is 1:(1-6), and more preferably 1:(2-4).

[0027] According to the present invention, in step (1), in order to obtain a better modification effect to facilitate the subsequent compounding of modified SiO2 with a water-soluble monomer, preferably, the weight ratio of the γ-methacryloxypropyltrimethoxysilane:SiO2 powder is 1:(1-4.5), and more preferably 1:(1.5-3.5).

[0028] According to the present invention, in step (1), the conditions of the modification process include: a temperature of 50-70°C, more preferably 60°C, and a time of 4.5 hours. The reaction system composed of the spherical SiO2 powder, ethanol solution, and vinyl trimethoxysilane modifies SiO2 at the temperature required for the modification process. In this process, the γ-methacryloxypropyl trimethoxysilane is first hydrated in the ethanol solution to replace the methyl group with the hydroxyl group. Therefore, the reaction should be carried out at the temperature required for the modification process for a sufficiently long time to make the γ-methacryloxypropyl trimethoxysilane modify the spherical SiO2 powder more thoroughly.

[0029] According to the present invention, in step (1), the operation of the modification process includes: first, adding an ethanol solution and deionized water in a three-necked flask according to a corresponding weight ratio, then adding spherical SiO2 powder, stirring at a speed of 250r / min for 15min, and adding γ-methacryloxypropyltrimethoxysilane when the solution is fully fused. At this speed, the solution pH is adjusted to 4.5 using a dilute hydrochloric acid standard solution and ultrasonicated for 45min. Then, the temperature is raised to 60°C and reacted in a water bath for 4.5h until the reaction is completed, to obtain modified SiO2 modified with γ-methacryloxypropyltrimethoxysilane.

[0030] According to a preferred embodiment of the present invention, in step (1), preferably, in order to fully mix the solution to achieve a better modification effect, a propeller stirring rod is used for stirring, wherein the three-blade stirring rod has a length of 400 mm, a blade span of 60 mm, and a rod diameter of 7 mm, to ensure that the dispersion and aggregation of the solution are balanced.

[0031] According to the present invention, in step (1), after the modification process is completed, a modified SiO2 product is obtained. After the reaction is completed, the product is centrifuged and washed with ethanol and deionized water to remove impurities, and then dried in a vacuum drying oven at 65°C for 24 hours to obtain modified SiO2.

[0032] In the present invention, the product is centrifuged after the modification process and washed with an ethanol solution. Specifically, the modified SiO2 product is mixed with an ethanol solution, and after being fully shaken, the low-speed centrifuge is adjusted to gear 3, and the product is centrifuged at a speed of 4000r / min for 30min. The above operation is repeated 3-4 times. To ensure that impurities are completely removed, the product is washed with ethanol twice after centrifugation. After the above operation is completed, the product is dried in a vacuum drying oven at 80°C for 20h. The lower solid obtained by centrifugation is the modified SiO2, and the upper clear liquid is the impurities.

[0033] According to the present invention, in step (2), the modified SiO2 is subjected to free radical polymerization with a water-soluble monomer by a reverse suspension polymerization method under the action of a dispersion medium, a dispersant, a crosslinking agent, an initiator, and other additives to obtain a SiO2 polymer microsphere material.

[0034] According to the present invention, in step (2), in order to achieve a better dispersion effect and reduce the synthesis cost, the dispersion medium is liquid paraffin, specifically, the relative density is 0.845, and the distillation temperature is greater than 300°C.

[0035] According to the present invention, in step (2), preferably, the dispersant is selected from one of Span-20, Span-40, Span-60 and Span-80, and more preferably Span-80.

[0036] Preferably, the water-soluble monomer is selected from at least two of acrylic acid, acrylamide, dimethyldiallylammonium chloride, sodium p-styrene sulfonate, sodium 3-mercapto-1-propanesulfonic acid, acryloylmorpholine, methacryloylethylsulfobetaine, and N-vinylpyrrolidone, and more preferably acrylamide, sodium p-styrene sulfonate, and N-vinylpyrrolidone.

[0037] Preferably, the cross-linking agent is selected from one of methylenebis(o-chloroaniline), N,N-methylenebisacrylamide and triallyl isocyanate, and more preferably N,N-methylenebisacrylamide.

[0038] Preferably, the initiator is selected from one of hydrogen peroxide, ferrous sulfate, benzoyl peroxide and ammonium persulfate, and more preferably ammonium persulfate.

[0039] According to the present invention, in step (2), the initiator ammonium persulfate is an ammonium persulfate solution with a mass fraction of 10%.

[0040] According to the present invention, in step (2), the additives include NH4Cl solution and NaOH solution to inhibit the hydrolysis of acrylamide. Specifically, the NH4Cl solution refers to an NH4Cl solution with a mass fraction of 10%, and the NaOH solution refers to a NaOH solution with a mass fraction of 15%.

[0041] According to the present invention, in step (2), in order to obtain the SiO2 polymer microsphere material with the best plugging effect, preferably, the weight ratio of the modified SiO2: liquid paraffin: Span-80: acrylamide: sodium p-styrene sulfonate: N-vinyl pyrrolidone: N,N-methylenebisacrylamide: ammonium persulfate: 10% NH4Cl solution: 15% NaOH solution is 1: (350-620): (18-28): (34-54): (25-35): (10-30): (2-6): (11-30): (2-7): (1-4), and further preferably is 1: (450-550): (19-23): (47-52): (28-32): (16-21): (2.8-3.6): (20-28): (3.8-6.6): (2.7-3.8).

[0042] According to the present invention, in step (2), the conditions of the polymerization process include: temperature of 50-75°C, more preferably 65°C, time of 4-7h, more preferably 6.5h.

[0043] According to the present invention, in step (2), the polymerization process operation includes: firstly, the modified SiO2, liquid paraffin and Span-80 in corresponding weight ratios are poured into a 250mL four-necked flask and fully stirred at a speed of 300r / min, and acrylamide, sodium p-styrene sulfonate, N-vinyl pyrrolidone, N,N-methylenebisacrylamide, ammonium persulfate, 10% NH4Cl solution and 15% NaOH solution are stirred at 300r / min for 30min according to the corresponding weight ratios, and then the solution is dripped into the three-necked flask with a dropping funnel at a dripping rate of 2mL / min, and after being fully stirred at a speed of 300r / min for 30min, nitrogen is passed and a condenser is connected, and then the temperature is raised to 65°C and an oil bath is reacted for 6.5h until the reaction is completed.

[0044] According to a preferred embodiment of the present invention, in (2), a four-necked flask is selected for the polymerization reaction, one of which is used for nitrogen, one is inserted with a thermometer to ensure that the temperature remains constant during the reaction, one is connected to a condenser to prevent the temperature from being too high during the reaction and the gas generated to cause excessive pressure in the four-necked flask, and the other is used to add the mixed solution. Secondly, it should be ensured that the polymerization reaction is carried out at a stable rotation speed to promote the formation of the SiO2 polymer microsphere structure.

[0045] According to the present invention, after the polymerization process is completed, a SiO2 polymer microsphere material is obtained, and the product is washed with an ethanol solution. Specifically, the product is mixed with a deethanol solution, and washed repeatedly for 5-7 times, and the obtained product is placed in a 60° C. vacuum drying oven and dried for 24 hours to obtain a product SiO2 polymer microsphere material.

[0046] The second aspect of the present invention provides a SiO2 polymer microsphere material prepared by the method described in the first aspect, wherein the particle size of the SiO2 polymer microsphere material ranges from 90 to 153 μm, which meets the plugging requirements of 120-200 μm cracks in terms of size.

[0047] According to the present invention, the SiO2 polymer microsphere material has amphiphilicity, so it can have good dispersibility in oil-based drilling fluid. Moreover, this amphiphilicity can play the role of surfactant in oil-based drilling fluid, and the SiO2 polymer microsphere material can stay at the oil-water interface of oil-based drilling fluid to enhance its stability. Due to its good deformability, the SiO2 polymer microsphere material can enter the formation cracks with different pore size ranges. When it encounters a crack with a pore size range smaller than the SiO2 polymer microsphere particle size, it can deform into the crack under the action of drilling hydraulic pressure difference and block the pore throat. When it encounters a crack with a pore size range greater than the SiO2 polymer microsphere particle size, it can absorb water and swell after entering the crack to block the pore throat. Moreover, since the SiO2 polymer microsphere surface contains hydrophilic groups, the microspheres can be connected by hydrogen bonds to prevent the invasion of oil-based drilling fluid.

[0048] The third aspect of the present invention provides the use of the SiO2 polymer microsphere material described in the second aspect as a plugging agent in oil-based drilling fluid.

[0049] The fourth aspect of the present invention provides an oil-based drilling fluid, which contains the SiO2 polymer microsphere material described in the second aspect.

[0050] According to the present invention, the oil-based drilling fluid comprises the following components: 100 parts by weight of base oil, 10-18 parts by weight of primary emulsifier, 4-10 parts by weight of secondary emulsifier, 1-9 parts by weight of wetting agent, 2-10 parts by weight of organic soil, 5-12 parts by weight of calcium oxide, 10-30 parts by weight of calcium chloride aqueous solution, 3-9 parts by weight of fluid loss reducer, 85-105 parts by weight of weighting agent, and 4-16 parts by weight of the SiO2 polymer microsphere material.

[0051] According to the present invention, the oil-based drilling fluid, on the basis of satisfying the above-mentioned composition, preferably, comprises the following components: 100 parts by weight of base oil, 12-16 parts by weight of primary emulsifier, 6-8 parts by weight of secondary emulsifier, 2-6 parts by weight of wetting agent, 6-10 parts by weight of organic soil, 5-7 parts by weight of calcium oxide, 22-28 parts by weight of calcium chloride aqueous solution, 4-8 parts by weight of fluid loss reducer, 88-100 parts by weight of weighting agent, and 3-9 parts by weight of the SiO2 polymer microsphere material.

[0052] According to the present invention, the base oil may be the commonly used oil-based drilling fluid base oil in the art, and the present invention has a relatively wide definition thereof, preferably diesel and / or mineral oil, further preferably mineral oil, and further preferably low-viscosity mineral oil. The mineral oil may be a conventional commercially available brand product, and the present invention has no particular limitation thereto.

[0053] Preferably, the primary emulsifier is selected from one of calcium cyclohexaneate, calcium alkylbenzene sulfonate, oleic acid, humic acid amide, and cyclohexane acid amide, and more preferably calcium cyclohexaneate.

[0054] Preferably, the secondary emulsifier is selected from one of Span-60, Span-80, acrylonitrile-butadiene-styrene, and humic acid amide, and more preferably Span-80.

[0055] Preferably, the wetting agent is selected from the group consisting of dodecyltrimethylammonium bromide, lecithin, and petroleum sulfonate, and more preferably is dodecyltrimethylammonium bromide.

[0056] Preferably, the organic soil is selected from oxidized asphalt, manganese dioxide, sulfonated asphalt, oleophilic clay obtained by the interaction of dodecyltrimethylammonium bromide and hydrophilic bentonite, and is further preferably oxidized asphalt.

[0057] Preferably, the concentration of the calcium chloride aqueous solution is 20-30 wt%, more preferably 25 wt% calcium chloride aqueous solution.

[0058] Preferably, the fluid loss reducer is selected from one of dimethyl disteadecyl ammonium chloride, polyalkylene polyamine fatty acid amide, and humic acid, and is more preferably dimethyl disteadecyl ammonium chloride.

[0059] Preferably, the weighting agent is selected from one of barite powder, limestone powder, calcium carbonate and iron ore powder, and is more preferably barite powder.

[0060] The oil-based drilling fluid provided by the present invention is amphiphilic and has excellent plugging ability, and can improve the success rate of plugging at one time.

[0061] The present invention will be described in detail by way of examples. The following are preparation examples, embodiments, comparative examples and test examples.

[0062] Preparation Example 1

[0063] (1-1) Add ethanol solution and deionized water in a weight ratio of 1:3 to a three-necked flask, then add 0.15 parts by weight of SiO2 powder (20nm, purity>99%), stir at 250r / min for 15min, and when the solution is fully fused, add γ-methacryloxypropyltrimethoxysilane in a weight ratio of γ-methacryloxypropyltrimethoxysilane to SiO2 powder of 1:2.5. At this speed, use a dilute hydrochloric acid standard solution to adjust the solution pH to 4.5 and ultrasonicate for 45min, then heat to 60°C in a water bath for 4.5h until the reaction is completed, to obtain modified SiO2.

[0064] (1-2) The product is centrifuged with a centrifuge and washed with ethanol after centrifugation. Specifically, the modified SiO2 product is mixed with an ethanol solution, and after being fully shaken, the low-speed centrifuge is adjusted to gear 3, and the product is centrifuged at a speed of 4000 r / min for 30 minutes. The above operation is repeated 3-4 times. To ensure that the impurities are completely removed, the product is washed with ethanol twice after centrifugation. After the above operation is completed, the product is dried in a vacuum drying oven at 80°C for 20 hours. The lower solid obtained by centrifugation is the modified SiO2, and the upper clear liquid is the impurities.

[0065] (1-3) First, the modified SiO2, liquid paraffin, and Span-80 in the corresponding weight ratio of 1:500:21 were poured into a 250 mL four-necked flask and fully stirred at 300 r / min. At the same time, acrylamide, sodium p-styrene sulfonate, N-vinyl pyrrolidone, N,N-methylenebisacrylamide, ammonium persulfate, 10% NH4Cl solution, and 15% NaOH solution in the weight ratio of 50:30:20:3.2:25:5:3.3 were stirred at 300 r / min for 30 min. Then, the solution was dripped into a three-necked flask with a dropping funnel at a dripping rate of 2 mL / min. After being fully stirred at 300 r / min for 30 min, nitrogen was passed and a condenser was connected. The temperature was then raised to 65°C in an oil bath for reaction for 6.5 h until the reaction was completed.

[0066] (1-4) After the polymerization process is completed, SiO2 polymer microsphere material is obtained, and the product is washed with an ethanol solution. Specifically, the product is mixed with a deethanol solution, and washed repeatedly for 5-7 times. The obtained product is placed in a vacuum drying oven at 60°C and dried for 24 hours to obtain a product SiO2 polymer microsphere material. (Recorded as S1).

[0067] Preparation Example 2

[0068] (2-1) Add ethanol solution and deionized water in a weight ratio of 1:2 to a three-necked flask, then add 0.15 parts by weight of SiO2 powder (20nm, purity>99%), stir at a speed of 250r / min for 15 minutes, and when the solution is fully fused, add γ-methacryloxypropyltrimethoxysilane in a weight ratio of γ-methacryloxypropyltrimethoxysilane:SiO2 powder of 1:1.5. At this speed, use a dilute hydrochloric acid standard solution to adjust the solution pH to 4.5 and ultrasonicate for 45 minutes, then heat to 60°C in a water bath for 4.5 hours until the reaction is completed, to obtain modified SiO2.

[0069] (2-2) The product is centrifuged with a centrifuge, and washed with ethanol and deionized water after centrifugation. Specifically, the modified SiO2 product is mixed with deionized water, and after being fully shaken, the low-speed centrifuge is adjusted to gear 2, and centrifuged at a speed of 4200 r / min for 20 minutes. The above operation is repeated until the pH of the supernatant is 7. To ensure that impurities are completely removed, the product is washed with ethanol and deionized water after centrifugation. After completing the above operation, it is dried in a vacuum drying oven at 65°C for 24 hours.

[0070] (2-3) First, the modified SiO2, liquid paraffin, and Span-80 in the corresponding weight ratio are poured into a 250 mL four-necked flask at a weight ratio of 1:450:19 and fully stirred at a speed of 300 r / min. At the same time, acrylamide, sodium p-styrene sulfonate, N-vinyl pyrrolidone, N,N-methylenebisacrylamide, ammonium persulfate, 10% NH4Cl solution, and 15% NaOH solution are stirred at a weight ratio of 47:28:16:2.8:20:3.8:2.7 at 300 r / min for 30 min. Then, the solution is dripped into a three-necked flask with a dropping funnel at a dripping rate of 2 mL / min. After fully stirring at a speed of 300 r / min for 30 min, nitrogen is passed and a condenser is connected. The temperature is then raised to 65°C in an oil bath for reaction for 6.5 h until the reaction is completed.

[0071] (2-4) After the polymerization process is completed, SiO2 polymer microsphere material is obtained, and the product is washed with an ethanol solution. Specifically, the product is mixed with a deethanol solution, and washed repeatedly for 5-7 times. The obtained product is placed in a vacuum drying oven at 60°C and dried for 24 hours to obtain a product SiO2 polymer microsphere material (denoted as S2).

[0072] Preparation Example 3

[0073] (3-1) Add ethanol solution and deionized water in a weight ratio of 1:4 to a three-necked flask, then add 0.15 parts by weight of SiO2 powder (20nm, purity>99%), stir at 250r / min for 15min, and when the solution is fully fused, add γ-methacryloxypropyltrimethoxysilane in a weight ratio of γ-methacryloxypropyltrimethoxysilane:SiO2 powder of 1:3.5. At this speed, use a dilute hydrochloric acid standard solution to adjust the solution pH to 4.5 and ultrasonicate for 45min, then heat to 60°C in a water bath for 4.5h until the reaction is completed, to obtain modified SiO2.

[0074] (3-2) The product is centrifuged with a centrifuge, and washed with ethanol and deionized water after centrifugation. Specifically, the modified SiO2 product is mixed with deionized water, and after being fully shaken, the low-speed centrifuge is adjusted to gear 2, and centrifuged at a speed of 4200 r / min for 20 minutes. The above operation is repeated until the pH of the supernatant is 7. To ensure that impurities are completely removed, the product is washed with ethanol and deionized water after centrifugation. After completing the above operation, it is dried in a vacuum drying oven at 65°C for 24 hours.

[0075] (3-3) First, the modified SiO2, liquid paraffin, and Span-80 in the corresponding weight ratio of 1:550:23 were poured into a 250mL four-necked flask and fully stirred at 300r / min. At the same time, acrylamide, sodium p-styrene sulfonate, N-vinyl pyrrolidone, N,N-methylenebisacrylamide, ammonium persulfate, 10% NH4Cl solution, and 15% NaOH solution in the weight ratio of 52:32:21:3.6:28:6.6:3.8 were stirred at 300r / min for 30min. Then, the solution was dripped into a three-necked flask with a dropping funnel at a dripping rate of 2mL / min. After being fully stirred at 300r / min for 30min, nitrogen was passed and a condenser was connected. The temperature was then raised to 65°C in an oil bath for reaction for 6.5h until the reaction was completed.

[0076] (3-4) After the polymerization process is completed, SiO2 polymer microsphere material is obtained, and the product is washed with an ethanol solution. Specifically, the product is mixed with a deethanol solution, and washed repeatedly for 5-7 times. The obtained product is placed in a vacuum drying oven at 60°C and dried for 24 hours to obtain a product SiO2 polymer microsphere material. (Recorded as S3).

[0077] Example 1

[0078] 100 parts by weight of low-viscosity mineral oil and 14 parts by weight of calcium cyclopentaneate were mixed and stirred at a stirring rate of 2000 r / min for 10 min, then 7 parts by weight of Span-80 were added and stirred at a stirring rate of 2000 r / min for 10 min, then 4 parts by weight of dodecyltrimethylammonium bromide were added and stirred at a stirring rate of 2000 r / min for 10 min, then 8 parts by weight of oxidized asphalt were added, and then 6 parts by weight of calcium oxide were added and stirred at a stirring rate of 2000 r / min for 10 min. n, then add 25 parts by weight of a 25% calcium chloride aqueous solution and stir at a stirring rate of 2000 r / min for 10 min, then add 6 parts by weight of dimethyl dioctadecyl ammonium chloride and stir at a stirring rate of 2000 r / min for 10 min, finally add 94 parts by weight of barite powder in 3 times and stir at a stirring rate of 2000 r / min for 30 min, finally add 6 parts by weight of plugging agent S1 and stir at a stirring rate of 2000 r / min for 10 min to obtain an oil-based drilling fluid (denoted as F1).

[0079] The components and contents of F1 are shown in Table 1.

[0080] Example 2-3

[0081] The method of Example 1 is followed, except that S2 and S3 are used as plugging agents, and other conditions are the same as those of Example 1. Oil-based drilling fluids (respectively denoted as F2 and F3) are obtained.

[0082] Example 4

[0083] 100 parts by weight of low-viscosity mineral oil and 12 parts by weight of calcium cyclopentaneate were mixed and stirred at a stirring rate of 2000 r / min for 10 min, then 6 parts by weight of Span-80 were added and stirred at a stirring rate of 2000 r / min for 10 min, then 2 parts by weight of dodecyltrimethylammonium bromide were added and stirred at a stirring rate of 2000 r / min for 10 min, then 6 parts by weight of oxidized asphalt were added, then 5 parts by weight of calcium oxide were added and stirred at a stirring rate of 2000 r / min for 10 min. n, then add 22 parts by weight of 25% calcium chloride aqueous solution and stir at a stirring rate of 2000 r / min for 10 minutes, then add 4 parts by weight of dimethyl dioctadecyl ammonium chloride and stir at a stirring rate of 2000 r / min for 10 minutes, finally add 88 parts by weight of barite powder in 3 times and stir at a stirring rate of 2000 r / min for 30 minutes, finally add 3 parts by weight of plugging agent S1 and stir at a stirring rate of 2000 r / min for 10 minutes to obtain an oil-based drilling fluid (recorded as F4).

[0084] The components and contents of F4 are shown in Table 1.

[0085] Embodiment 5-6

[0086] The method of Example 4 was followed, except that S2 and S3 were used as plugging agents, and other conditions were the same as those of Example 4. Oil-based drilling fluids (respectively denoted as F5 and F6) were obtained.

[0087] Example 7

[0088] 100 parts by weight of low-viscosity mineral oil and 16 parts by weight of calcium naphthenate were mixed and stirred at a stirring rate of 2000 r / min for 10 min, then 8 parts by weight of Span-80 were added and stirred at a stirring rate of 2000 r / min for 10 min, then 6 parts by weight of dodecyltrimethylammonium bromide were added and stirred at a stirring rate of 2000 r / min for 10 min, then 10 parts by weight of oxidized asphalt were added, then 7 parts by weight of calcium oxide were added and stirred at a stirring rate of 2000 r / min for 10 min. 0min, then add 28 parts by weight of 25% calcium chloride aqueous solution and stir at a stirring rate of 2000r / min for 10min, then add 8 parts by weight of dimethyl dioctadecyl ammonium chloride and stir at a stirring rate of 2000r / min for 10min, finally add 100 parts by weight of barite powder in 3 times and stir at a stirring rate of 2000r / min for 30min, finally add 9 parts by weight of plugging agent S1 and stir at a stirring rate of 2000r / min for 10min to obtain oil-based drilling fluid (denoted as F7).

[0089] The components and contents of F7 are shown in Table 1.

[0090] Embodiment 8-9

[0091] The method of Example 7 was followed, except that S2 and S3 were used as plugging agents, respectively, and other conditions were the same as those of Example 7. Oil-based drilling fluids (respectively denoted as F8 and F9) were obtained.

[0092] Comparative Example 1

[0093] The method of Example 1 is followed, except that the plugging agent S1 is not added, and other conditions are the same as those of Example 1. An oil-based drilling fluid (denoted as DF1) is obtained.

[0094] Comparative Example 2

[0095] The method of Example 1 is followed, except that the modified SiO2 prepared in step (1-1) of Preparation Example 1 is used as a plugging agent (denoted as S4), and other conditions are the same as those of Example 1. An oil-based drilling fluid (denoted as DF2) is obtained.

[0096] Comparative Example 3

[0097] The method of Example 2 is followed, except that the modified SiO2 prepared in step (1-1) of Preparation Example 2 is used as a plugging agent (denoted as S5), and other conditions are the same as those of Example 2. An oil-based drilling fluid (denoted as DF3) is obtained.

[0098] Comparative Example 4

[0099] The method of Example 3 was followed, except that the modified SiO2 prepared in step (1-1) of Preparation Example 3 was used as a plugging agent (denoted as S6), and the other conditions were the same as those of Example 1. An oil-based drilling fluid (denoted as DF4) was obtained.

[0100] Comparative Example 5

[0101] The method of Example 1 is followed, except that S1 is replaced by spherical SiO2 powder, and other conditions are the same as those of Example 1. An oil-based drilling fluid (denoted as DF5) is obtained.

[0102] Comparative Example 6

[0103] The method of Example 1 is followed, except that S1 is replaced with micron-sized calcium carbonate, a common laboratory plugging agent, and other conditions are the same as those of Example 1. A water-based drilling fluid (denoted as DF6) is obtained.

[0104] Table 1

[0105]

[0106]

[0107] Table 2

[0108]

[0109]

[0110] Test Case

[0111] The expansion ratio test of the SiO2 polymer microsphere material prepared in Preparation Examples S1-S3 was carried out to evaluate its expansion capacity, and the plugging performance test of the oil-based drilling fluid prepared in Examples F1-F9 and Comparative Examples DF1-DF6 was carried out. GB / T16783.2-2012 "Field Test of Drilling Fluids in the Petroleum and Natural Gas Industry Part 2: Oil-Based Drilling Fluids", the drilling fluids prepared in Examples 1-9 and Comparative Examples 1-6 were evaluated. In the following test examples,

[0112] Apparent viscosity (AV, mPa·s), plastic viscosity (PV, mPa·s), and dynamic shear force (YP, Pa) were measured using a six-speed rotational viscometer according to the method in GB / T 16783.2-2012;

[0113] The demulsification voltage (Es, V) is measured using an electrical stability tester according to the method in GB / T 16783.2-2012;

[0114] High temperature and high pressure filtration loss (HTHP, mL) was measured using a high temperature and high pressure filtration instrument according to the method in GB / T16783.2-2012;

[0115] The sand bed plugging loss (mL) was measured using a medium-pressure sand bed filter loss tester;

[0116] The manufacturer of the contact angle tester is Chengdu Snow Leopard Technology Co., Ltd., model SDC-350;

[0117] The manufacturer of the six-speed rotational viscometer is Meike Company, and the model is ZNN-D6B electronic six-speed rotational viscometer;

[0118] The manufacturer of the electrical stability tester is Meike Company, and the model is DWY-2 electrical stability tester;

[0119] The manufacturer of the high temperature and high pressure filter loss instrument is Meike Company, and the model is GGS42-2A high temperature and high pressure filter loss instrument-PID electronic temperature control;

[0120] The manufacturer of the leak plugging instrument is Meike Company, and the model is QD-2 portable leak plugging instrument.

[0121] 1. Expansion ratio test

[0122] 1 mL of S1-S3 obtained in the preparation example was placed in a 50 mL pressure tube and recorded as V1. Deionized water was added until the scale line reached 50 mL. The tube was taken out after standing at different temperatures for 24 hours. The test temperatures were 25°C, 65°C, and 95°C. The volume change of the microspheres during this period was observed, and the expansion ratio was calculated as follows:

[0123]

[0124] Among them, V t is the oil absorption ratio after expansion of preparation examples S1-S3, V0 is the volume before oil absorption, V t , V0 unit is mL.

[0125] Table 3

[0126]

[0127] As can be seen from Table 3, as the temperature rises, the oil absorption ratio of Preparation Examples S1-S3 gradually increases. This is because as the temperature rises, the interaction between the secondary bonds weakens, and the curled macromolecular chains gradually stretch, resulting in an increase in the molecular thermodynamics, an enhanced dispersion of water molecules, and more and more water molecules entering the polymer. As can be seen from Table 3, the expansion ratio of Preparation Example S1 is the highest, while the expansion ratio of S2 is the lowest. This is because the amount of cross-linking agent and sodium p-styrene sulfonate is too much. Too much cross-linking agent leads to excessive cross-linking density, and the macromolecular chain is not easy to unfold. Sodium p-styrene sulfonate contains benzene rings, which will produce a steric hindrance effect and hinder the absorption of water molecules.

[0128] 2. Contact angle test

[0129] The purified and dried SiO2 polymer microspheres were pressurized at 10 MPa for 5 min at room temperature to obtain a smooth film. The contact angles of white oil and distilled water with the film were measured under air conditions.

[0130] The results are shown in Table 4

[0131]

[0132]

[0133] It can be seen from Table 4 that SiO2 polymer microspheres are hydrophilic and lipophilic because there are many hydrophilic functional groups such as amide groups and sulfonic acid groups on the surface of the microspheres. In addition, due to the use of reverse suspension polymerization, an oil film is produced on the surface of the polymer, so the microspheres also have good dispersibility in the oil environment.

[0134] 2. Leakage plugging performance test

[0135] The plugging performance test is mainly carried out by a sand bed filtration evaluation device and a self-made micro-crack plugging simulation device. Specifically, the sand bed filtration evaluation device has a specific operation method: fill the container with quartz sand of different particle sizes to the set position, inject the embodiments F1-F9 and the comparative examples DF1-DF6 respectively, tighten and pressurize, inject it into the simulated leakage channel under pressure, measure the filtration loss, and test its pressure-bearing plugging performance in the cracks. Among them, since the rocks in the shale layer are mostly quartz sand, quartz sand is used to simulate the cracks in the underground rock formation, and the particle size distribution of the quartz sand used is 150-180μm, 180-250μm, and 250-380μm. Among them, the filtration loss under 380-550μm, 550-700μm, and 700-830μm is recorded as FL1, FL2, and FL3 respectively.

[0136] Specifically, the operation method of the self-made micro-crack plugging simulation device is as follows: after assembling the micro-crack simulation rigid seam plate, install it at the lower end of the inner cylinder of the GGS42-2A high-temperature and high-pressure filtration tester kettle, then install the lower part of the tank according to the normal steps, calibrate the crack width with a standard thickness gauge aluminum foil, and then pour the prepared drilling fluid slurry into the tank. Among them, the crack width of the micro-crack device is set to 150μm, 220μm, and 300μm, respectively, and the oil-based drilling fluids F1-F9 prepared in Examples 1-9 and the oil-based drilling fluids DF1-DF6 prepared in Comparative Examples 1-6 are tested at a temperature of 160°C and a pressure difference of 3.5MPa to test their filtration loss. The filtration loss at 100μm, 150μm, and 220μm is recorded as FL4, FL5, and FL6, respectively.

[0137] Table 5 Oil-based drilling fluid sand bed filtration and plugging performance test of Examples F1-F9 and Comparative Examples DF1-DF6

[0138]

[0139]

[0140] Table 6 Leakage plugging performance test of oil-based drilling fluids F1-F9 prepared in Examples 1-9 and oil-based drilling fluids DF1-DF6 prepared in Comparative Examples 1-6 in micro-crack plugging simulation device

[0141] <![CDATA[FL3 / mL]]> <![CDATA[FL4 / mL]]> <![CDATA[FL5 / mL]]> F1 6 7.4 8.6 F2 7.6 8.2 9.8 F3 7.2 7.8 8.8 F4 7.8 8.6 10 F5 9.8 10.2 11.2 F6 10.4 11.8 12.4 F7 13.2 14.2 15.4 F8 14.2 15.2 16.4 F9 13.8 14.8 15.2 DF1 16 18.8 20 DF2 16.8 18.6 17.8 DF3 15.8 16.6 18.4 DF4 15 16.2 17 DF5 19.8 25.6 26 DF6 22 25 28

[0142] It can be seen from Table 5 and Table 6 that as the amount of SiO2 polymer microspheres increases, the intrusion depth of the sand bed test and the filtration loss of the high temperature and high pressure test will decrease. When the amount is too low, an effective plugging layer cannot be formed in the leakage channel, and the microspheres cannot interact with each other. When the amount of SiO2 polymer microspheres is too much, the macromolecular chains on the surface of the microspheres may entangle with each other, making the cross-linking density larger, and bonding occurs before reaching the leakage channel, resulting in poor plugging performance. When the amount of SiO2 polymer microsphere plugging material is 6% (based on the weight of low viscosity mineral oil), a thin and dense mud cake can be formed. Since the surface of the microspheres contains amide groups and sulfonic acid groups, the polymers can interact with each other, making their arrangement in the pores more compact, achieving a better plugging effect.

[0143] 3. Compatibility test

[0144] Prepare oil-based drilling fluid base slurry A (100 parts by weight of low-viscosity mineral oil + 14 parts by weight of primary emulsifier + 7 parts by weight of secondary emulsifier + 4 parts by weight of wetting agent + 8 parts by weight of organic soil + 6 parts by weight of calcium oxide + 25 parts by weight of calcium chloride solution + 6 parts by weight of filtrate reducer + 94 parts by weight of filtrate reducer), then add 6% (based on the weight of low-viscosity mineral oil) of SiO2 polymer microsphere material S1 obtained in Preparation Example 1 to the above-mentioned base slurry A to obtain oil-based drilling fluid B.

[0145] The rheological parameters and demulsification voltage of oil-based drilling fluid slurry A and oil-based drilling fluid B at room temperature were tested respectively, and the results are shown in Table 7.

[0146] Drilling Fluid AV(mPa·s) PV (mPa·s) YP(Pa) Es(V) A 69 38 4.5 874 B 72 43 5.7 1140

[0147] It can be seen from Table 7 that the addition of the SiO2 polymer microsphere plugging agent of the present invention has little effect on the rheological parameters of the oil-based drilling fluid. Moreover, the demulsification voltage is increased after the addition of the SiO2 polymer microsphere plugging agent, which indicates that the SiO2 polymer microsphere plugging agent can effectively maintain the electrical stability of the oil-based drilling fluid. This is because the amphiphilicity of the SiO2 polymer microspheres allows them to be adsorbed on the oil-water contact interface of the oil-based drilling fluid, thereby improving the emulsion stability of the system.

Claims

1. A SiO2 polymer microsphere, a preparation method and application thereof, and an oil-based drilling fluid, characterized in that: The method includes: (1) contacting SiO2 with a silane coupling agent under acidic conditions to modify it, thereby obtaining modified SiO2; (2) The modified SiO2 was reacted with three water-soluble monomers by reverse suspension polymerization to obtain modified SiO2 polymer microsphere material.

2. The method according to claim 1, wherein: In step (1), the weight ratio of the ethanol solution to deionized water is 1:(1-6), more preferably 1:(2-4); Wherein, in step (1), the weight ratio of silane coupling agent:SiO2 powder is 1:(1-4.5), and more preferably 1:(1.5-3.5).

3. The method according to claim 1, wherein: In step (2), the weight ratio of modified SiO2: liquid paraffin: dispersant: cross-linking agent: initiator: 10% NH4Cl solution: 15% NaOH solution: water-soluble monomer is 1: (350-620): (18-28): (2-6): (11-30): (2-7): (1-4): (69-119), and more preferably 1: (450-550): (19-23): (2.8-3.6): (20-28): (3.8-6.6): (2.7-3.8): (91-105).

4. The method according to any one of claims 1 to 3, wherein: In step (1), the silane coupling agent is selected from one of vinyl tri(b-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, and methacryloxypropyl trimethoxysilane, and more preferably γ-methacryloxypropyl trimethoxysilane.

5. The method according to any one of claims 1 to 3, wherein: In step (2), preferably, the dispersant is selected from one of Span-20, Span-40, Span-60, and Span-80, and more preferably Span-80; Preferably, the water-soluble monomer is selected from at least two of acrylic acid, acrylamide, dimethyldiallylammonium chloride, sodium p-styrene sulfonate, sodium 3-mercapto-1-propanesulfonic acid, acryloylmorpholine, methacryloylethylsulfobetaine, and N-vinylpyrrolidone, and more preferably acrylamide, sodium p-styrene sulfonate, and N-vinylpyrrolidone; Preferably, the cross-linking agent is selected from one of methylenebis(o-chloroaniline), N,N-methylenebisacrylamide, and triallyl isocyanate, and more preferably N,N-methylenebisacrylamide; Preferably, the cross-linking agent is selected from one of N,N-methylenebisacrylamide, methylenebis(o-chloroaniline), and cyclohexanone peroxide, and more preferably N,N-methylenebisacrylamide; Preferably, the initiator is selected from one of hydrogen peroxide, ferrous sulfate, benzoyl peroxide and ammonium persulfate, and more preferably ammonium persulfate.

6. The method according to any one of claims 1 to 4, wherein: In step (1), the conditions of the modification process include: a temperature of 50-70° C., more preferably 60° C.; a washing method of centrifugation and washing with ethanol and deionized water to remove impurities; Preferably, in step (2), the conditions of the polymerization process include: a temperature of 50-75°C, more preferably 65°C, and a time of 4-7h, more preferably 6.5h; Preferably, in step (2), after the polymerization process is completed, a SiO2 polymer microsphere material is obtained, and after the reaction is completed, the product is washed with an ethanol solution.

7. A SiO2 polymer microsphere material obtained by the preparation method according to any one of claims 1 to 5, wherein: The particle size range of the SiO2 polymer microsphere material is 90-153 μm.

8. Use of the SiO2 polymer microsphere material according to claim 6 as a plugging agent in oil-based drilling fluid.

9. An oil-based drilling fluid comprising the SiO2 polymer microsphere material according to claim 6.

10. The oil-based drilling fluid comprises the following components: 100 parts by weight of base oil, 10-18 parts by weight of primary emulsifier, 4-10 parts by weight of secondary emulsifier, 1-9 parts by weight of wetting agent, 2-10 parts by weight of organic soil, 5-12 parts by weight of calcium oxide, 10-30 parts by weight of calcium chloride aqueous solution, 3-9 parts by weight of fluid loss reducer, 85-105 parts by weight of weighting agent, and 4-16 parts by weight of SiO2 polymer microsphere material; Preferably, the oil-based drilling fluid comprises the following components: 100 parts by weight of base oil, 12-16 parts by weight of primary emulsifier, 6-8 parts by weight of secondary emulsifier, 2-6 parts by weight of wetting agent, 6-10 parts by weight of organic soil, 5-7 parts by weight of calcium oxide, 22-28 parts by weight of calcium chloride aqueous solution, 4-8 parts by weight of fluid loss reducer, 88-100 parts by weight of weighting agent, and 3-9 parts by weight of the SiO2 polymer microsphere material; According to the present invention, the base oil may be a commonly used oil-based drilling fluid base oil in the art, and the present invention has a relatively wide range of limitations, preferably diesel and / or mineral oil, more preferably mineral oil, and even more preferably low-viscosity mineral oil. The mineral oil may be a conventional commercially available brand product, and the present invention has no particular limitations on this. Preferably, the primary emulsifier is selected from one of calcium cyclohexaneate, calcium alkylbenzene sulfonate, oleic acid, humic acid amide, and cyclohexane acid amide, and more preferably calcium cyclohexaneate; Preferably, the secondary emulsifier is selected from one of Span-60, Span-80, acrylonitrile-butadiene-styrene, and humic acid amide, and more preferably Span-80; Preferably, the wetting agent is selected from one of dodecyltrimethylammonium bromide, lecithin, and petroleum sulfonate, and more preferably is dodecyltrimethylammonium bromide; Preferably, the organic soil is selected from oxidized asphalt, manganese dioxide, sulfonated asphalt, oleophilic clay obtained by the interaction of dodecyltrimethylammonium bromide and hydrophilic bentonite, and is further preferably oxidized 5 asphalt; Preferably, the concentration of the calcium chloride aqueous solution is 20-30wt%, more preferably 25wt% calcium chloride aqueous solution; Preferably, the fluid loss reducer is selected from one of dimethyl disteadecyl ammonium chloride, polyalkylene polyamine fatty acid amide, and humic acid, and is further preferably dimethyl disteadecyl ammonium chloride; Preferably, the weighting agent is selected from one of barite powder, limestone powder, calcium carbonate and iron ore powder, and is more preferably barite powder.

Citation Information

Patent Citations

  • Lost circulation material with soft outside and rigid inside and preparation method thereof

    CN113528101A

  • High-temperature-resistant and saturated-salt-resistant plugging filtrate reducer and preparation method thereof

    CN114686190A

  • Plugging agent suitable for leakage prevention and plugging of hard and brittle formation and cement paste system

    CN116333701A

  • Core-shell structure microsphere blocking agent for oil-based drilling fluid and preparation method of core-shell structure microsphere blocking agent

    CN117777353A

  • High temperature and high salinity-resistant complementarily rigid-flexible plugging agent and method for preparing the same and water-based drilling fluid and use thereof