Preparation method of polyaldehydes ester capable of being chemically circulated, product of polyaldehydes ester and chemical circulation method of polyaldehydes ester
By alternately copolymerizing linear aldehyde with a specific structure of six-membered cyclic anhydride, polyaldehyde esters with chemical cyclability and fully alternating structures were prepared, which solved the problem of difficulty in copolymerizing linear aldehydes and achieved efficient polymer degradation and recovery.
Patent Information
- Application Number
- CN202310653438.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-05
AI Technical Summary
In the prior art, linear aldehydes are difficult to undergo homopolymerization or copolymerization reactions due to the low polymerization enthalpy change, which limits the preparation and application of polyaldehyde esters.
Linear aldehydes are used to alternately copolymerize with six-membered cyclic anhydrides and/or seven-membered cyclic anhydrides that have both macrocyclic tension and small steric hindrance. Through Lewis acid or protonic acid catalysis, a chemically cyclable and fully alternating structure is prepared. Polyaldehyde esters.
The linear aldehyde copolymerization reaction is achieved, and polyaldehyde esters with excellent degradation properties and high molecular weight are prepared, which can be completely depolymerized and converted into raw materials under mild conditions, achieving closed-loop recovery of polymers.
Smart Images

Figure CN119081040A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a preparation method of chemically cyclable polyaldehyde ester, a product thereof and a chemical recycling method. Background Art
[0002] Since Hermann Staudinger first proposed the concept of polymers with covalent bonds as the core in 1920, polymer science has experienced a century of development, and polymers have become an indispensable material in social development. While synthetic polymer materials have brought great convenience to mankind, the contradiction with the sustainable development of human society is becoming increasingly prominent: first, the raw materials rely on non-renewable fossil resources, and a large amount of CO2 is emitted in industrial production; second, carbon chain polymer materials with carbon-carbon bonds as the main chain are extremely stable, and it takes hundreds or even thousands of years to degrade into small molecules under natural conditions.
[0003] Cyclic anhydrides are common compounds that can be prepared by heating the corresponding (bio-based) dibasic acid and dehydrating the molecule. Cyclic anhydride-epoxide anion copolymerization is an emerging method for synthesizing polyesters, which has the advantages of atom economy, easy structure control, and mild polymerization conditions. To date, more than 20 types of cyclic anhydrides and epoxides have been reported to participate in the copolymerization, and more than 400 types of synthesized polyesters have been reported.
[0004] A Chinese patent document with application publication number CN 113861395 A discloses a polyester containing an acetal group in the main chain and a preparation method thereof, which is prepared by alternating copolymerization of cyclic acetal and cyclic anhydride as raw materials. Unlike cyclic acetal, linear aldehyde is a linear molecule without ring tension. As a monomer that is abundant in nature and has a wide range of biological sources, such as lily of the valley aldehyde, perillaldehyde, and citrus aldehyde, it is considered to be one of the monomers with the most development potential in the 21st century. The polymer prepared from aldehyde is expected to replace traditional petroleum-based materials with good development prospects. However, unfortunately, in current research, except for formaldehyde, which has been widely studied and confirmed to be able to undergo cationic homopolymerization to prepare polyoxymethylene and copolymerize with other cyclic acetals to prepare copolymerized formaldehyde (In Polyoxymethylene Handbook, 2014; pp 21-51), other linear aldehydes are difficult or even impossible to undergo homopolymerization or copolymerization due to their lower polymerization enthalpy change (Macromolecules 2021, 54, 9165-9173). Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention discloses a method for successfully preparing polyaldehyde ester using linear aldehyde and cyclic anhydride as raw materials. The method is simple and controllable, and the prepared product is a fully alternating polyaldehyde ester with a clear chain structure. More importantly, the polyaldehyde ester prepared by the method has chemical recyclability and can be completely depolymerized and converted into raw materials through simple pyrolysis, thereby realizing the chemical cycle of the polyaldehyde ester.
[0006] The specific technical solutions are as follows:
[0007] A method for preparing a chemically recyclable polyaldehyde ester comprises:
[0008] The chemically cyclable polyaldehyde ester is prepared by using linear aldehyde and cyclic anhydride as raw materials and Lewis acid or protonic acid as catalyst through alternating copolymerization;
[0009] The linear aldehyde has the following general structural formula:
[0010]
[0011] In the formula, R is selected from a branched or straight-chain alkyl group having 1 to 20 carbon atoms, a branched or straight-chain alkenyl group having 2 to 20 carbon atoms, a branched or straight-chain alkynyl group having 2 to 20 carbon atoms, a branched or straight-chain terpene group having 5 to 20 carbon atoms, a branched or straight-chain cycloalkyl group having 3 to 20 carbon atoms, an aromatic group having 5 to 20 carbon atoms, and the above groups containing one or more heteroatoms selected from O, S, N, Si, P, F, Cl, Br, and I;
[0012] When R is selected from a branched alkenyl or straight alkenyl having 2 to 20 carbon atoms, the alkenyl cannot form a conjugation with the double bond in the aldehyde group;
[0013] When R is selected from a branched or straight chain alkynyl group having 2 to 20 carbon atoms, the alkynyl group cannot form conjugation with the double bond in the aldehyde group;
[0014] The cyclic anhydride is selected from six-membered cyclic anhydride and / or seven-membered cyclic anhydride;
[0015] If the six-membered cyclic anhydride has a substituent, the substituent cannot be a directly connected alicyclic substituent;
[0016] If the seven-membered cyclic anhydride has a substituent, the substituent cannot be a directly connected alicyclic substituent.
[0017] The inventors have found through a large number of experiments that only when six-membered cyclic anhydrides and / or seven-membered cyclic anhydrides with special structures having both large ring tension and small steric hindrance are screened, the polymerization enthalpy change of the cyclic anhydride ring-opening polymerization can compensate for the entropy change of the linear aldehyde polymerization process, thereby initiating a copolymerization reaction and achieving the copolymerization of the linear aldehyde.
[0018] Therefore, the present invention has certain requirements for the structure of the cyclic anhydride. First, a six-membered cyclic anhydride and / or a seven-membered cyclic anhydride with large ring tension is selected. At the same time, in order to ensure less steric hindrance, it is further required that if the cyclic anhydride has a substituent, the substituent cannot be a directly connected alicyclic substituent.
[0019] Preferably, the linear aldehyde is selected from one or more of a straight-chain alkyl with a carbon number of 1 to 20, cyclohexanecarboxaldehyde, benzaldehyde, 2,3-dichlorobenzaldehyde, and lily of the valley aldehyde; these preferred aldehyde monomers have a wide range of chemical or biological sources, are easily obtained in large quantities, and are convenient to store and transport. It is particularly important that these preferred aldehyde monomers have simple structures and are easier to polymerize thermodynamically.
[0020] Preferably, the cyclic anhydride is selected from one or more of glutaric anhydride, diglycolic anhydride, thiodiglycolic anhydride, 3-methylglutaric anhydride, 3,3-dimethylglutaric anhydride, 2,2-dimethylglutaric anhydride, 3-isobutylglutaric anhydride, hexafluoroglutaric anhydride, and adipic anhydride. These preferred cyclic anhydride monomers are cheap and readily available common industrial products, and are convenient for storage and transportation. At the same time, these preferred cyclic anhydride monomers have good reactivity and excellent effect with the linear aldehyde monomer.
[0021] Preferably, the molar ratio of the cyclic anhydride to the linear aldehyde is 0.1 to 10:1; more preferably 0.5 to 1.5:1, preferably within this range, the polymer product can be guaranteed to have an alternation degree of ≥ 99%. More preferably, it is 1.0 to 1.5:1, and the conversion rate of the polymerization reaction is higher under this more preferred molar ratio, and the molecular weight of the prepared polymer product is higher.
[0022] Preferably, the molar ratio of the catalyst to the cyclic anhydride is 1:5 to 10000; more preferably 1:50 to 7500, preferably within this range, the polymerization can be ensured to have a higher polymerization efficiency. More preferably, it is 1:100 to 7500, and further preferably 1:1000 to 7500; as the above molar ratio is continuously optimized, the conversion rate of the polymerization reaction is higher, and a polymer product with a higher molecular weight can be prepared.
[0023] Preferably, the alternating copolymerization reaction is carried out at -20 to 60°C under autogenous pressure for 0.05 to 12 hours; more preferably, the temperature of the alternating copolymerization reaction is -20 to 25°C; more preferably, -20 to 0°C. It has been found through experiments that the particularity of this polymerization reaction is that low temperature is more conducive to the polymerization reaction; as the polymerization reaction temperature decreases, the conversion rate of the polymerization reaction is higher, and a higher molecular weight polymerization product can be prepared.
[0024] Further experiments revealed that in this polymerization reaction, when R is selected from an aromatic group with a carbon number of 5 to 20, and an aromatic group with a carbon number of 5 to 20 containing one or more heteroatoms selected from O, S, N, Si, P, F, Cl, Br, and I, the polymerization reaction requires a lower temperature (-20 to 0°C).
[0025] In the alternating copolymerization reaction, the Lewis acid is selected from one or more of BF3, B(C6F5)3, InCl3, InBr3, SnCl4, AlCl3, SbCl5, PF5, CF3SO3Et, and Ph3CPF6;
[0026] The protonic acid is selected from one or more of HBF4, HClO4, CF3COOH, CF3SO4H, FSO4H, and concentrated sulfuric acid.
[0027] Preferably, the catalyst is selected from InCl3 and / or InBr3. Experiments have shown that, compared with other catalyst types, the preferred catalyst has higher catalytic activity and can produce a polymer product with a higher molecular weight under the same conditions.
[0028] The present invention also discloses a chemically recyclable polyaldehyde ester prepared according to the above method:
[0029] The chemically cyclable polyaldehyde ester has a fully alternating structure, an ester chain content of ≥99%, and an aldehyde group is present in each repeating unit.
[0030] The invention also discloses a method for chemical recycling of polyaldehyde ester, wherein the chemically cyclable polyaldehyde ester prepared according to the method is heated to 160-180° C. under vacuum conditions for thermal decomposition.
[0031] Preferably, the vacuum is evacuated to a vacuum degree of <0.1 KPa.
[0032] The chemically recyclable polyaldehyde ester prepared by the above method can be quantitatively degraded by the above simple and mild pyrolysis, with a conversion rate of >99% and an aldehyde yield of ≥88%.
[0033] Preferably, the selected chemically recyclable polyaldehyde ester has a linear aldehyde substituent selected from an aromatic group having 5 to 20 carbon atoms, or an aromatic group having 5 to 20 carbon atoms containing one or more heteroatoms selected from O, S, N, Si, P, F, Cl, Br, and I.
[0034] Experiments have found that chemically recyclable polyaldehyde esters prepared using linear aldehydes containing aromatic groups, aromatic heterocycles, or aromatic groups or aromatic heterocycles containing substituents as raw materials are easier to achieve chemical recycling, require lower pyrolysis temperatures, shorter times, and have higher aldehyde yields (≥95%).
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention is based on a large number of experimental studies and realizes the cationic alternating copolymerization of linear aldehyde monomers and cyclic anhydride monomers for the first time. Since the two monomer raw materials are easy to prepare, have a wide range of biological sources and are cheap and easy to obtain, the polymerization reaction has great practical value.
[0037] (2) The polyaldehyde ester prepared by the present invention has a fully alternating structure and a regular structure, and has broad application prospects in food packaging, biology and electronic fields.
[0038] (3) The polyaldehyde ester prepared by the present invention has excellent degradation performance. Under static vacuum and relatively mild conditions (160-180° C.), it can be converted from polymer to monomer, completing the closed-loop recovery of the monomer. The polymer conversion rate is >99% and the monomer recovery rate is >88%. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The polyaldehyde ester prepared in Example 1 1 H NMR spectrum;
[0040] Figure 2 The polyaldehyde ester prepared in Example 1 13 C NMR spectrum;
[0041] Figure 3 The polyaldehyde ester prepared in Example 2 1 H NMR spectrum;
[0042] Figure 4 The polyaldehyde ester prepared in Example 2 13 C NMR spectrum;
[0043] Figure 5 The polyaldehyde ester prepared in Example 3 1 H NMR spectrum;
[0044] Figure 6 The polyaldehyde ester prepared in Example 3 13 C NMR spectrum;
[0045] Figure 7 The polyaldehyde ester prepared in Example 4 1 H NMR spectrum;
[0046] Figure 8 The polyaldehyde ester prepared in Example 4 13 C NMR spectrum;
[0047] Fig. 9 The polyaldehyde ester prepared in Example 6 1H NMR spectrum;
[0048] Fig.10 The polyaldehyde ester prepared in Example 6 13 C NMR spectrum;
[0049] Fig.11 The polyaldehyde ester prepared in Example 7 1 H NMR spectrum;
[0050] Fig.12 The polyaldehyde ester prepared in Example 7 13 C NMR spectrum;
[0051] Fig.13 The polyaldehyde ester prepared in Example 8 1 H NMR spectrum;
[0052] Fig.14 The polyaldehyde ester prepared in Example 8 13 C NMR spectrum;
[0053] Fig.15 For the polyaldehyde ester prepared in Example 9 1 H NMR spectrum;
[0054] Fig.16 For the polyaldehyde ester prepared in Example 9 13 C NMR spectrum. DETAILED DESCRIPTION
[0055] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.
[0056] Example 1 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0057] Before the polymerization reaction, remove moisture from a 10mL Shrek tube at 110°C for 2 hours and cool to room temperature in a glove box; add a certain mass of InBr3, acetaldehyde, glutaric anhydride and 1mL of dichloromethane to the Shrek tube in sequence. The molar ratio of InBr3 / acetaldehyde / glutaric anhydride is 1 / 100 / 100. React at 25°C under autogenous pressure for 0.1h. After the reaction is completed, the crude product is first dissolved in dichloromethane, and then the polymer is precipitated in a mixture of 100mL of methanol / sodium phenolate (sodium phenolate molar concentration is 5%), washed three times, and vacuum dried to constant weight. The molecular weight and molecular weight distribution of the polymer are determined by gel chromatography, and the test results are shown in Table 1.
[0058] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 1 As shown, 13 CNMR spectrum Figure 2Observation Figure 1 and Figure 2 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0059] Degradation performance test:
[0060] The sublimator was placed at 110°C for about 12 hours to remove moisture and cooled to room temperature in a glove box; the polyaldehyde ester prepared in this embodiment was added to the sublimator, and the sublimator was sealed and placed under a vacuum pump to evacuate for 30 minutes until the vacuum degree was <0.1KPa to remove air and then the device was sealed. It was placed at 180°C and reacted under autogenous pressure for 12 hours. After the reaction was completed, the lower layer of raw materials and the upper layer of sublimation products in the sublimator were taken and weighed respectively. Its purity was tested by nuclear magnetic resonance, and the test results are shown in Table 2.
[0061] Comparative Example 1
[0062] Before the polymerization reaction, a 10 mL Shrek tube was dehydrated at 110°C for 2 hours and cooled to room temperature in a glove box; a certain amount of InBr3, acetaldehyde, maleic anhydride and 1 mL of dichloromethane were added to the Shrek tube in sequence. The molar ratio of InBr3 / acetaldehyde / maleic anhydride was 1 / 100 / 100. The reaction was carried out at 25°C under autogenous pressure for 12 hours.
[0063] The product after the reaction was a colorless liquid. No precipitation was generated in a 100 mL mixture of methanol and sodium phenolate (sodium phenolate molar concentration was 5%). It was preliminarily determined that no polymerization reaction occurred in the system. The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0064] According to the test results, it can be further determined that acetaldehyde does not copolymerize with maleic anhydride, a representative of five-membered cyclic anhydrides.
[0065] Comparative Example 2
[0066] The preparation process is substantially the same as that in Comparative Example 1, except that the reaction system is placed at 100° C. under autogenous pressure for 12 hours.
[0067] The product after the reaction was a colorless liquid. No precipitation was generated in a 100 mL mixture of methanol and sodium phenolate (sodium phenolate molar concentration was 5%). It was preliminarily determined that no polymerization reaction occurred in the system. The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0068] According to the test results, it can be determined that even when the reaction temperature is increased, acetaldehyde and maleic anhydride, a representative of five-membered cyclic anhydrides, still do not undergo copolymerization reaction.
[0069] Comparative Example 3
[0070] The preparation process is basically the same as that in Example 1, except that:
[0071] Acetaldehyde was replaced with an equal molar amount of cinnamaldehyde, and the reaction system was placed at 25° C. under autogenous pressure for 12 hours.
[0072] The product after the reaction was a colorless liquid. No precipitation was generated in a 100 mL mixture of methanol and sodium phenolate (sodium phenolate molar concentration was 5%). It was preliminarily determined that no polymerization reaction occurred in the system. The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0073] According to the test results, it can be determined that no copolymerization reaction occurs between glutaric anhydride and cinnamaldehyde having conjugated unsaturated bonds.
[0074] Comparative Example 4
[0075] The preparation process is basically the same as that in Example 1, except that:
[0076] Acetaldehyde was replaced with an equal mole of furanaldehyde, and the reaction system was placed at 25° C. under autogenous pressure for 12 hours.
[0077] The product after the reaction was a colorless liquid. No precipitation was generated in a 100 mL mixture of methanol and sodium phenolate (sodium phenolate molar concentration was 5%). It was preliminarily determined that no polymerization reaction occurred in the system. The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0078] According to the test results, it can be determined that no copolymerization reaction occurs between glutaric anhydride and furanaldehyde having conjugated unsaturated bonds.
[0079] Example 2 Cyclohexanecarboxaldehyde / glutaric anhydride alternating copolymerization to form fully alternating polyaldehyde ester
[0080] The preparation process is basically the same as that in Example 1, except that:
[0081] Acetaldehyde was replaced with an equal mole of cyclohexanecarboxaldehyde, and the reaction system was placed at 25° C. under autogenous pressure for 0.5 hours.
[0082] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0083] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 3 As shown, 13 CNMR spectrum Figure 4 Observation Figure 3 and Figure 4 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0084] Example 3 Alternating copolymerization of eicosanal / glutaric anhydride to form fully alternating polyaldehyde ester
[0085] The preparation process is basically the same as that in Example 1, except that:
[0086] Acetaldehyde was replaced with an equal mole of eicosanal, and the reaction system was placed at 25° C. under autogenous pressure for 0.5 hours.
[0087] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0088] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 5 As shown, 13 CNMR spectrum Figure 6 Observation Figure 5 and Figure 6 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0089] Example 4 Alternating copolymerization of benzaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0090] The preparation process is basically the same as that in Example 1, except that:
[0091] Acetaldehyde was replaced with an equal mole of benzaldehyde, and the reaction system was placed at 0°C and reacted under autogenous pressure for 0.5 hours.
[0092] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0093] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 7 As shown, 13 CNMR spectrum Figure 8 Observation Figure 7 and Figure 8 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0094] Degradation performance test:
[0095] The sublimator was placed at 110°C for about 12 hours to remove moisture and cooled to room temperature in a glove box; the polyaldehyde ester prepared in this embodiment was added to the sublimator, and the sublimator was sealed and placed under a vacuum pump to evacuate for 30 minutes until the vacuum degree was <0.1KPa to remove air and then the device was sealed. It was placed at 160°C and reacted under autogenous pressure for 3 hours. After the reaction was completed, the lower layer of raw materials and the upper layer of sublimation products in the sublimator were taken and weighed respectively. Its purity was tested by nuclear magnetic resonance, and the test results are shown in Table 2.
[0096] Example 5 Alternating copolymerization of benzaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0097] The preparation process is basically the same as that in Example 4, except that:
[0098] The reaction system was placed at 25°C under autogenous pressure for 0.5 hours.
[0099] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0100] Example 62,3-Dichlorobenzaldehyde / glutaric anhydride alternating copolymerization to form fully alternating polyaldehyde ester
[0101] The preparation process is basically the same as that in Example 1, except that:
[0102] Acetaldehyde was replaced with an equal molar amount of 2,3-dichlorobenzaldehyde, and the reaction system was placed at -20°C under autogenous pressure for 12 hours.
[0103] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0104] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig. 9 As shown, 13 CNMR spectrum Fig.10 Observation Fig. 9 and Fig.10 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0105] Degradation performance test:
[0106] The sublimator was placed at 110°C for about 12 hours to remove moisture and cooled to room temperature in a glove box; the polyaldehyde ester prepared in this embodiment was added to the sublimator, and the sublimator was sealed and placed under a vacuum pump to evacuate for 30 minutes until the vacuum degree was <0.1KPa to remove air and then the device was sealed. It was placed at 160°C and reacted under autogenous pressure for 3 hours. After the reaction was completed, the lower layer of raw materials and the upper layer of sublimation products in the sublimator were taken and weighed respectively. Its purity was tested by nuclear magnetic resonance, and the test results are shown in Table 2.
[0107] Example 7 Alternating copolymerization of lilysulphate / glutaric anhydride to form fully alternating polyaldehyde ester
[0108] The preparation process is basically the same as that in Example 1, except that:
[0109] Acetaldehyde was replaced with an equal mole of lily of the valley aldehyde, and the reaction system was placed at 25° C. under autogenous pressure for 0.5 hours.
[0110] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0111] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig.11 As shown, 13 CNMR spectrum Fig.12 Observation Fig.11 and Fig.12 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0112] Example 8 Alternating copolymerization of acetaldehyde / 3-methylglutaric anhydride to form fully alternating polyaldehyde ester
[0113] The preparation process is basically the same as that in Example 1, except that:
[0114] Glutaric anhydride was replaced with an equal molar amount of 3-methylglutaric anhydride, and the reaction system was placed at 25° C. under autogenous pressure for 0.5 hours.
[0115] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0116] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig.13 As shown, 13 CNMR spectrum Fig.14 Observation Fig.13 and Fig.14 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0117] Comparative Example 5
[0118] The preparation process is basically the same as that in Example 1, except that:
[0119] The glutaric anhydride was replaced with an equal molar amount of 3,3-tetramethyleneglutaric anhydride, and the reaction system was placed at 25° C. under autogenous pressure for 12 hours.
[0120] The product after the reaction was a colorless liquid. No precipitation was generated in a 100 mL mixture of methanol and sodium phenolate (sodium phenolate molar concentration was 5%). It was preliminarily determined that no polymerization reaction occurred in the system. The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0121] According to the test results, it can be determined that there is no copolymerization reaction between acetaldehyde and 3,3-tetramethyleneglutaric anhydride with large steric hindrance.
[0122] Comparative Example 6
[0123] The preparation process is basically the same as that in Example 1, except that:
[0124] Glutaric anhydride was replaced with an equal molar amount of 1,1-cyclohexyldiacetic anhydride, and the reaction system was placed at 25° C. under autogenous pressure for 12 hours.
[0125] The product after the reaction was a colorless liquid. No precipitation was generated in a 100 mL mixture of methanol and sodium phenolate (sodium phenolate molar concentration was 5%). It was preliminarily determined that no polymerization reaction occurred in the system. The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0126] According to the test results, it can be determined that there is no copolymerization reaction between acetaldehyde and 1,1-cyclohexyldiacetic anhydride with large steric hindrance.
[0127] Example 9 Alternating copolymerization of acetaldehyde / adipic anhydride to form fully alternating polyaldehyde ester
[0128] The preparation process is basically the same as that in Example 1, except that:
[0129] Glutaric anhydride was replaced with an equal mole of adipic anhydride, and the reaction system was placed at 25° C. under autogenous pressure for 0.5 hours.
[0130] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0131] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig.15 As shown, 13 CNMR spectrum Fig.16 Observation Fig.15 and Fig.16 It can be seen that there is no peak corresponding to the polyaldehyde chain segment in the figure, indicating that the obtained product has a completely alternating chain segment structure.
[0132] Embodiment 10-11 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0133] The preparation process is basically the same as that in Example 1, except that:
[0134] The catalyst was replaced with an equal mole of BF3 and an equal mole of TfOH, respectively.
[0135] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0136] Example 12 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0137] The preparation process is basically the same as that in Example 1, except that:
[0138] The molar ratio of InBr3 / acetaldehyde / glutaric anhydride was replaced to 1 / 50 / 50.
[0139] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0140] Example 13 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0141] The preparation process is basically the same as that in Example 1, except that:
[0142] The molar ratio of InBr3 / acetaldehyde / glutaric anhydride was replaced with 1 / 1000 / 1000, and the reaction system was placed at 25°C under autogenous pressure for 6 hours.
[0143] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0144] Example 14 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0145] The preparation process is basically the same as that in Example 1, except that:
[0146] The molar ratio of InBr3 / acetaldehyde / glutaric anhydride was replaced with 1 / 7500 / 7500, and the reaction system was placed at 25°C under autogenous pressure for 12 hours.
[0147] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0148] Examples 15-16 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde esters
[0149] The preparation process is basically the same as that in Example 1, except that:
[0150] The molar ratios of InBr3 / acetaldehyde / glutaric anhydride were replaced to 1 / 50 / 100 and 1 / 150 / 100, respectively.
[0151] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0152] Examples 17-19 Alternating copolymerization of acetaldehyde / glutaric anhydride to form fully alternating polyaldehyde esters
[0153] The preparation process is basically the same as that in Example 1, except that:
[0154] The reaction temperature of the reaction system was changed to 0°C, 40°C and 60°C respectively.
[0155] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0156] Table 1
[0157]
[0158]
[0159]
[0160] 1 M n : number average molecular weight, determined by gel permeation chromatography; 2 PDI: Molecular weight distribution, determined by gel permeation chromatography.
[0161] Table 2
[0162]
[0163] The applicant declares that the present invention illustrates the detailed method of the present invention through the above embodiments, but the present invention is not limited to the above detailed method.
Claims
1. A method for preparing a chemically recyclable polyaldehyde ester, characterized in that: include: The chemically cyclable polyaldehyde ester is prepared by using linear aldehyde and cyclic anhydride as raw materials and Lewis acid or protonic acid as catalyst through alternating copolymerization; The linear aldehyde has the following general structural formula: In the formula, R is selected from a branched or straight-chain alkyl group having 1 to 20 carbon atoms, a branched or straight-chain alkenyl group having 2 to 20 carbon atoms, a branched or straight-chain alkynyl group having 2 to 20 carbon atoms, a branched or straight-chain terpene group having 5 to 20 carbon atoms, a branched or straight-chain cycloalkyl group having 3 to 20 carbon atoms, an aromatic group having 5 to 20 carbon atoms, and the above groups containing one or more heteroatoms selected from O, S, N, Si, P, F, Cl, Br, and I; When R is selected from a branched alkenyl or straight alkenyl having 2 to 20 carbon atoms, the alkenyl cannot form a conjugation with the double bond in the aldehyde group; When R is selected from a branched or straight chain alkynyl group having 2 to 20 carbon atoms, the alkynyl group cannot form conjugation with the double bond in the aldehyde group; The cyclic anhydride is selected from six-membered cyclic anhydride and / or seven-membered cyclic anhydride; If the six-membered cyclic anhydride has a substituent, the substituent cannot be a directly connected alicyclic substituent; If the seven-membered cyclic anhydride has a substituent, the substituent cannot be a directly connected alicyclic substituent.
2. The method for preparing a chemically recyclable polyaldehyde ester according to claim 1, wherein: The molar ratio of the cyclic anhydride to the linear aldehyde is 0.1 to 10:1; The molar ratio of the catalyst to the cyclic anhydride is 1:5 to 10000; The alternating copolymerization reaction is carried out at -20 to 60° C. under autogenous pressure for 0.05 to 12 hours.
3. The method for preparing chemically recyclable polyaldehyde ester according to claim 1, characterized in that: The Lewis acid is selected from one or more of BF3, B(C6F5)3, InCl3, InBr3, SnCl4, AlCl3, SbCl5, PF5, CF3SO3Et, and Ph3CPF6; The protonic acid is selected from one or more of HBF4, HClO4, CF3COOH, CF3SO4H, FSO4H, and concentrated sulfuric acid.
4. The method for preparing chemically recyclable polyaldehyde ester according to claim 1, characterized in that: The linear aldehyde is selected from one or more of a straight-chain alkyl having a carbon number of 1 to 20, cyclohexanecarboxaldehyde, benzaldehyde, 2,3-dichlorobenzaldehyde, and lily of the valley aldehyde; The cyclic anhydride is selected from one or more of glutaric anhydride, diglycolic anhydride, thiodiglycolic anhydride, 3-methylglutaric anhydride, 3,3-dimethylglutaric anhydride, 2,2-dimethylglutaric anhydride, 3-isobutylglutaric anhydride, hexafluoroglutaric anhydride, and adipic anhydride.
5. The method for preparing chemically recyclable polyaldehyde ester according to claim 4, characterized in that: The molar ratio of cyclic anhydride to linear aldehyde is 0.5 to 1.5:1; The molar ratio of the catalyst to the cyclic anhydride is 1:50-7500.
6. The method for preparing chemically recyclable polyaldehyde ester according to claim 5, characterized in that: The catalyst is selected from InCl3 and / or InBr3.
7. The method for preparing chemically recyclable polyaldehyde ester according to claim 1, characterized in that: The alternating copolymerization reaction is carried out at -20 to 25°C under autogenous pressure for 0.1 to 12 hours.
8. A chemically recyclable polyaldehyde ester prepared by the method according to any one of claims 1 to 7, characterized in that: The chemically cyclable polyaldehyde ester has a fully alternating structure, an ester chain content of ≥99%, and an aldehyde group is present in each repeating unit.
9. A method for chemical recycling of polyaldehyde esters, characterized in that, The chemically recyclable polyaldehyde ester according to claim 8 is heated to 160-180° C. under vacuum conditions for thermal decomposition.
10. The method for chemical recycling of polyaldehyde ester according to claim 9, characterized in that:The substituents of the linear aldehyde used in the preparation process of the chemically recyclable polyaldehyde ester are selected from aromatic groups with carbon numbers of 5 to 20, or aromatic groups with carbon numbers of 5 to 20 containing one or more heteroatoms selected from O, S, N, Si, P, F, Cl, Br, and I.
Citation Information
Patent Citations
Polyester with main chain containing acetal group and preparation method of polyester
CN113861395A
Aldehyde copolymers and their preparation
US3277058A
Method for producing polyacetal-polyesters from cyclic anhydrides and aldehydes
WO2015135948A1