Rigid molecular chain introduced polyurethane foam material and preparation method thereof
By introducing polyols and hydroxyl molecular chain substances with longer molecular chains into polyurethane foaming materials, the impact resistance and support performance of the material is improved, and the existing polyurethane foaming materials are easily damaged and insufficient support during impact are solved. The problem is applicable to a wider range of blocking construction scenarios.
Patent Information
- Application Number
- CN202411292973.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polyurethane foaming materials are prone to damage during impact and lack support performance, which limits their application in sealing construction.
By introducing polyols with longer molecular chains and rigid molecular chain substances containing hydroxyl groups react with isocyanate, the impact resistance and support properties of polyurethane foaming materials are improved.
The generated polyurethane foaming material has stronger impact resistance and better support performance, solving the problems of easy damage to hard bubbles and insufficient support of soft bubbles. It is suitable for more application scenarios such as distribution boxes in power systems. Cable seal.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of plugging and filling materials, and particularly relates to a polyurethane foam material introduced with rigid molecular chains and a preparation method thereof. Background Art
[0002] Polyurethane foam is a polymer-based material with a large number of cellular structures created through physical or chemical methods. Polyurethane foam is a polymer composed of repeating urethane segments, produced by the reaction of isocyanates and polyols. The unique cellular structure of polyurethane foam imparts a range of excellent properties, including low density, thermal and acoustic insulation, high specific strength, cushioning, and thermal insulation. Therefore, it is widely used in packaging, industry, agriculture, transportation, military, aerospace, and daily necessities.
[0003] Polyurethane foam materials are mainly divided into two series: rigid foam and soft foam. Currently, rigid foam is mainly used for sealing construction. However, the current rigid foam is easily damaged when impacted, which requires repair and easily causes secondary construction. Soft foam is mainly used for filling various dolls, cars and furniture. It does not have good supporting performance during the sealing construction process, so its application in the field of hole sealing is limited.
[0004] Based on this, it is necessary to provide a polyurethane foam material with introduced rigid molecular chains and a preparation method thereof, so that the prepared polyurethane foam material can have good supporting performance and good impact resistance to solve the above problems. Summary of the Invention
[0005] In order to make up for the deficiencies of the prior art and obtain a polyurethane foam material with certain supporting performance and impact resistance, the present invention provides a polyurethane foam material with introduced rigid molecular chains and a preparation method thereof.
[0006] The present invention solves the above technical problems through the following solutions: Based on a polyurethane foam material with an introduced rigid molecular chain and its preparation method, a reinforcing agent is added to enhance the supporting performance of the polyurethane foam material, and a polyol with a longer molecular chain is selected to improve the impact resistance of the polyurethane foam material.
[0007] The reinforcing agent is a rigid molecular chain substance containing hydroxyl groups. Through the reaction of hydroxyl groups and isocyanate groups, the resulting polyurethane foam material can have good supporting properties, thereby achieving the effect of improving the supporting properties of the polyurethane foam material.
[0008] The reaction between the polyol with a longer molecular chain and the isocyanate makes the resulting polyurethane foam material have excellent impact resistance.
[0009] A polyurethane foam material with a rigid molecular chain and a preparation method thereof include the following steps: (1) The polyol, chain extender, catalyst, foam stabilizer and enhancer were weighed in a certain proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0010] (2) A certain proportion of foaming agent was weighed and added to solution A, and stirred at 800 rpm at 20°C to obtain solution B after 5 minutes.
[0011] (3) Add isocyanate to solution B in a certain proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0012] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0013] The beneficial technical effects achieved by the present invention include at least the following: The polyurethane foam material of the present invention, which incorporates a rigid molecular chain, uses a rigid molecular chain substance containing hydroxyl groups as a reinforcing agent. The hydroxyl groups and isocyanate groups undergo a condensation reaction, resulting in a polyurethane foam material with improved support properties compared to conventional polyurethane soft foam materials, thereby resolving the drawback of polyurethane soft foams having insufficient support under certain circumstances. The reaction between polyols and isocyanates of selected molecular chain lengths results in a foam material with enhanced impact resistance compared to conventional polyurethane rigid foams, thereby resolving the drawback of polyurethane rigid foams being easily damaged by impact. DETAILED DESCRIPTION
[0014] The present invention is further described below by way of examples, which are only used to explain the present invention and do not constitute any limitation thereto.
[0015] Example 1 A polyurethane foam material into which rigid molecular chains are introduced, comprising the following components by mass percentage: Propylene glycol 40%, triethanolamine 0.4%, dibutyltin dilaurate 2%, dimethyl silicone oil 5%, hydroxy silicone oil 2.6%, ethanol 4%, diphenylmethane isocyanate 46%.
[0016] Based on a polyurethane foam material with a rigid molecular chain introduced and a preparation method thereof, the invention specifically includes the following steps: (1) Propylene glycol, triethanolamine, dibutyltin dilaurate, dimethyl silicone oil and hydroxy silicone oil were weighed in proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0017] (2) Weigh a proportion of ethanol and add it to solution A. Stir the mixture at 800 rpm at 20°C to obtain solution B after 5 minutes.
[0018] (3) Add diphenylmethane isocyanate to solution B in proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0019] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0020] Example 2 A polyurethane foam material into which rigid molecular chains are introduced, comprising the following components by mass percentage: Propylene glycol 43%, triethanolamine 1.4%, stannous octoate 2.5%, dimethyl silicone oil 5%, hydroxy silicone oil 2.6%, ethanol 4%, diphenylmethane isocyanate 41.5%.
[0021] Based on a polyurethane foam material with a rigid molecular chain introduced and a preparation method thereof, the invention specifically includes the following steps: (1) Propylene glycol, triethanolamine, stannous octoate, dimethyl silicone oil and hydroxy silicone oil were weighed in proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0022] (2) Weigh a proportion of ethanol and add it to solution A. Stir the mixture at 800 rpm at 20°C to obtain solution B after 5 minutes.
[0023] (3) Add diphenylmethane isocyanate to solution B in proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0024] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0025] Example 3 A polyurethane foam material into which rigid molecular chains are introduced, comprising the following components by mass percentage: Ethylene glycol 45%, triethanolamine 1.4%, stannous octoate 3%, dimethyl silicone oil 4%, hydroxy silicone oil 2.6%, ethanol 3%, diphenylmethane isocyanate 41%.
[0026] Based on a polyurethane foam material with a rigid molecular chain introduced and a preparation method thereof, the invention specifically includes the following steps: (1) Ethylene glycol, triethanolamine, stannous octoate, dimethyl silicone oil and hydroxy silicone oil were weighed in proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0027] (2) Weigh a proportion of ethanol and add it to solution A. Stir the mixture at 800 rpm at 20°C to obtain solution B after 5 minutes.
[0028] (3) Add diphenylmethane isocyanate to solution B in proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0029] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0030] Example 4 A polyurethane foam material into which rigid molecular chains are introduced, comprising the following components by mass percentage: Ethylene glycol 22%, propylene glycol 20%, triethanolamine 1.4%, stannous octoate 3%, dimethyl silicone oil 4%, hydroxy silicone oil 2.6%, ethanol 3.5%, water 2.5%, diphenylmethane isocyanate 41%.
[0031] Based on a polyurethane foam material with a rigid molecular chain introduced and a preparation method thereof, the invention specifically includes the following steps: (1) Ethylene glycol, propylene glycol, triethanolamine, stannous octoate, dimethyl silicone oil and hydroxy silicone oil were weighed in proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0032] (2) Weigh and add ethanol and water in proportion to solution A, stir at 800 rpm at 20°C, and obtain solution B after 5 minutes.
[0033] (3) Add diphenylmethane isocyanate to solution B in proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0034] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0035] Example 5 A polyurethane foam material into which rigid molecular chains are introduced, comprising the following components by mass percentage: Ethylene glycol 20%, propylene glycol 20%, triethanolamine 1%, stannous octoate 3.5%, dimethicone 4%, phenol 2.5%, ethanol 3.5%, water 2.5%, diphenylmethane isocyanate 43%.
[0036] Based on a polyurethane foam material with a rigid molecular chain introduced and a preparation method thereof, the invention specifically includes the following steps: (1) Ethylene glycol, propylene glycol, triethanolamine, stannous octoate, dimethyl silicone oil and phenol were weighed in proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0037] (2) Weigh and add ethanol and water in proportion to solution A, stir at 800 rpm at 20°C, and obtain solution B after 5 minutes.
[0038] (3) Add diphenylmethane isocyanate to solution B in proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0039] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0040] Example 6 A polyurethane foam material into which rigid molecular chains are introduced, comprising the following components by mass percentage: Propylene glycol 20%, triethanolamine 1%, stannous octoate 3.5%, dimethicone 4%, phenol 2.5%, ethanol 3.5%, water 2.5%, diphenylmethane isocyanate 23%, diisocyanate 20%.
[0041] Based on a polyurethane foam material with a rigid molecular chain introduced and a preparation method thereof, the invention specifically includes the following steps: (1) Propylene glycol, triethanolamine, stannous octoate, dimethyl silicone oil and phenol were weighed in proportion, added together in sequence, and stirred at 800 rpm for 30 minutes to obtain solution A.
[0042] (2) Weigh and add ethanol and water in proportion to solution A, stir at 800 rpm at 20°C, and obtain solution B after 5 minutes.
[0043] (3) Add diphenylmethane isocyanate and diisocyanate to solution B in proportion, stir for 15 seconds, and then pour into a mold to obtain a polyurethane foam material.
[0044] (4) The polyurethane foam material obtained in the previous step is placed in an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with rigid molecular chains.
[0045] Table 1 Compression test data of samples made with different ratios of dimethyl silicone oil and hydroxy silicone oil
[0046] Compared with traditional polyurethane foam materials, the polyurethane foam material with introduced rigid molecular chains of the present invention can adapt to more application scenarios. The previous hard foam of polyurethane foam material is easily damaged, and the soft foam can only be used as a surface sealing material in many scenarios due to the lack of certain support, which is not conducive to simple and lightweight operations on its surface. In the cable sealing operation of the distribution box in the power system, multiple procedures of construction are often required, and the most basic construction is the sealing of polyurethane foam materials. Due to the above-mentioned problems, the previous foam material has a difficult construction process, complicated and tedious procedures, and the construction process requires carefulness and is time-consuming and labor-intensive. The present invention provides a suitable solution based on this application scenario.
[0047] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A polyurethane foam material with a rigid molecular chain introduced therein and a method for preparing the same, characterized in that: Calculated by mass percentage, it includes the following components: 30% to 50% of polyol, 0.01% to 2% of chain extender, 0.01% to 5% of catalyst, 2% to 10% of foam stabilizer, 1% to 10% of enhancer, 2% to 8% of blowing agent and 30% to 50% of isocyanate.
2. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The polyol includes a mixture of one or more of ethylene glycol, propylene glycol, caprylyl glycol and glycerol.
3. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The chain extender includes one or more of dimethylethylenediamine, triethanolamine and ethanolamine.
4. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The silicon catalyst includes a mixture of one or more of dibutyltin dilaurate, triethylenediamine, dibutyltin behenamide and stannous octoate.
5. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The foam stabilizer comprises a mixture of one or more of dimethyl silicone oil, polyvinyl alcohol and polyacrylamide.
6. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The reinforcing agent includes a mixture of one or more of polyvinyl alcohol, hydroxy silicone oil and phenol.
7. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The foaming agent comprises a mixture of one or more of ethanol, water, ammonia and epoxidized butylene glycol polyurethane.
8. The polyurethane foam material with rigid molecular chains introduced therein and the preparation method thereof according to claim 1, characterized in that: The isocyanate includes a mixture of one or more of diphenylmethane isocyanate, diisocyanate and polyether diisocyanate.
9. A polyurethane foam material with a rigid molecular chain introduced therein and a method for preparing the same as claimed in any one of claims 1 to 8, characterized in that The preparation method comprises the following steps: 1) taking out and weighing a polyol, a chain extender, a catalyst, a foam stabilizer and an enhancer in a certain proportion, adding them together in sequence and stirring them to obtain a solution A; 2) taking out and weighing a certain proportion of a foaming agent and adding it to the solution A, stirring it at a temperature of 20°C, and obtaining a solution B after 5 minutes; 3) adding isocyanate in a certain proportion to the solution B, stirring it, and then pouring it into a mold to obtain a polyurethane foam material; 4) putting the polyurethane foam material obtained in the previous step into an oven at 50°C for aging for 2 hours to obtain a polyurethane foam material with a rigid molecular chain.
Citation Information
Patent Citations
Polyurethane material for mops
CN112321791A
Anti-condensation high-flame-retardancy polyurethane foaming material and preparation method thereof
CN113667088A
Polyurethane microcellular foam material for railway under-rail backing plate and preparation method thereof
CN114591485A
High-strength controllable foaming material as well as preparation method and application thereof
CN114933687A
Polyurethane foam material as well as preparation method and application thereof
CN116333251A