Flame-retardant antibacterial polyurethane as well as preparation method and application thereof

By grafting the phospho-containing silicon quaternary ammonium salt in polyurethane materials, using its flame retardant and antibacterial components on the surface of the material, the problem of insufficient flame retardant and antibacterial properties of the polyurethane materials is solved, and the efficient flame retardant and antibacterial properties of the material is achieved. The effect is simplified and the preparation process is suitable for industrial production.

CN119081051APending Publication Date: 2024-12-06GUANGZHOU CITY POLYTECHNIC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411232945.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing polyurethane materials lack flame retardant and antibacterial properties, making it difficult to delay combustion in fire and prevent bacteria from growing. The preparation process is complicated and not environmentally friendly.

Method used

The phosphorus-containing silicon quaternary ammonium salt is combined with polyurethane, and the phosphorus-containing silicon quaternary ammonium salt is grafted on the polyurethane branch chain, and the flame retardant and antibacterial properties are enhanced by the phosphorus, silicon, nitrogen and halogen components on the surface of the material, and the flame retardant and antibacterial properties are enhanced in the The reaction is carried out under an inert gas atmosphere to simplify the preparation process.

Benefits of technology

It realizes excellent flame retardant properties and antibacterial properties of polyurethane materials, reduces material combustion and bacterial growth, and has a simple and environmentally friendly preparation process, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005026818970000021
    Figure BDA0005026818970000021
  • Figure BDA0005026818970000032
    Figure BDA0005026818970000032
  • Figure BDA0005026818970000041
    Figure BDA0005026818970000041
Patent Text Reader

Abstract

The invention belongs to the field of high polymer materials, and particularly relates to flame-retardant antibacterial polyurethane as well as a preparation method and application thereof. The flame-retardant antibacterial polyurethane is prepared from the following raw materials in parts by weight: 5 to 40 parts of quaternary ammonium salt containing phosphorus and silicon, 100 parts of polyether polyol or polyester polyol, 17.5 to 30 parts of diisocyanate, 0.1 to 0.5 part of organic metal catalyst, 0 to 5 parts of chain extender, 0.1 to 2.0 parts of defoaming agent and 3 to 17 parts of curing agent. The preparation method comprises the following steps: firstly, preparing a phosphorus-silicon-containing quaternary ammonium salt, and then grafting the phosphorus-silicon-containing quaternary ammonium salt on a polyurethane branch chain. The quaternary ammonium salt containing phosphorus and silicon simultaneously contains four flame-retardant components of phosphorus, nitrogen, silicon and halogen, and can synergistically enhance the flame-retardant property of polyurethane. The flame-retardant antibacterial polyurethane disclosed by the invention integrates the properties of the phosphorus-containing flame retardant, the organosilicon quaternary ammonium salt and the polyurethane, so that the polyurethane has excellent flame-retardant property and antibacterial property on the basis of keeping the original advantages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and specifically relates to a flame retardant and antibacterial polyurethane and a preparation method and application thereof. Background Art

[0002] Polyurethane is a common polymer material that can be used in many fields such as home appliances, toys, communication products, kitchen utensils, clothing, building materials, medical materials, etc. In recent years, electric vehicle combustion, residential, factory and other building fires have occurred from time to time. Polyurethane products are not flame retardant, and polyurethane foam is even flammable. Giving polyurethane materials a flame retardant function can delay the occurrence of fires or reduce the losses caused by fires to a greater extent. In addition, during the use or storage of polyurethane products, bacteria will grow under suitable temperature and humidity conditions, which is not good for people's health and also affects its use effect and service life. Therefore, it is very necessary to introduce flame retardancy and antibacterial properties into polyurethane products so that they have both flame retardancy and antibacterial properties to meet market demand.

[0003] Phosphorus-based flame retardants are a class of highly efficient, stable, and widely used flame retardants. Introducing phosphorus-containing compounds into polyurethane can prepare flame-retardant polyurethane materials. Silicone is an environmentally friendly and efficient flame retardant with good thermal stability. At the same time, it has a low heat release rate during thermal decomposition, does not release toxic gases, and produces less smoke. In addition, silicone has good hydrophobicity, which can reduce the water absorption of the material surface, which is conducive to keeping the material surface dry, thereby reducing the growth and reproduction of microorganisms such as bacteria. Quaternary ammonium salts are a class of broad-spectrum, highly efficient bactericides. Modifying polyurethane with quaternary ammonium salts can effectively enhance the antibacterial properties of polyurethane. In addition, quaternary ammonium salts contain nitrogen and halogens, both of which can improve flame retardant efficiency. Therefore, combining phosphorus-containing compounds, silicones, and quaternary ammonium salts to prepare phosphorus-containing silicon quaternary ammonium salts, and using them to modify polyurethane, can simultaneously enhance the flame retardancy and antibacterial ability of polyurethane materials. At present, there are many studies on flame-retardant polyurethanes or antibacterial polyurethanes with single properties, but there are few studies on flame-retardant and antibacterial polyurethanes with dual properties. For example, Ge Tiejun and others from Shenyang University of Chemical Technology introduced nitrogen and phosphorus elements into polyols to improve the oxygen index of polyurethane foam. The results showed that with the increase of phosphorus and nitrogen content, the oxygen index of polyurethane foam increased significantly, from 19.1% to 26.5%, and the flame retardancy was greatly improved. However, the preparation process of this scheme is complicated, has high requirements on reaction conditions, uses many reagents, is not environmentally friendly, and the prepared polyurethane has a single performance, only flame retardancy but no antibacterial properties.

[0004] Zhang Wentao and others from Zhejiang University used self-made dihydroxyl-terminated agent MTS, 2,4,6-tris(3-chloropropyl)-2,4,6-trimethyl-cyclotrisiloxane and octamethylcyclotetrasiloxane (D4) to obtain chloropropyl-containing dihydroxyl-terminated polysiloxane through ring-opening copolymerization, and then introduced quaternary ammonium salt groups with bactericidal properties into the silicone chain through quaternization reaction, and synthesized polyurethane through the reaction of hydroxyl and isocyanate; the results showed that when the quaternary ammonium salt content was 20%, the bactericidal rate of polyurethane against Gram-positive bacteria and Gram-negative bacteria could reach more than 90%. However, the polyurethane prepared by this method has a single function, a complicated preparation process, and solvent pollution. Summary of the invention

[0005] In order to solve the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a flame retardant antibacterial polyurethane.

[0006] Another object of the present invention is to provide a method for preparing the flame retardant and antibacterial polyurethane.

[0007] Another object of the present invention is to provide an application of the flame retardant and antibacterial polyurethane.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A flame retardant antibacterial polyurethane, the preparation raw materials of which include: 5-40 parts by weight of phosphorus-containing silicon quaternary ammonium salt, 100 parts by weight of polyether polyol or polyester polyol, 17.5-30 parts by weight of diisocyanate, 0.1-0.5 parts by weight of organic metal catalyst, 0-5 parts by weight of chain extender, 0.1-2.0 parts by weight of defoamer and 3-17 parts by weight of curing agent.

[0010] Preferably, the structural formula of the phosphorus-containing silicon quaternary ammonium salt is as shown in formula (1):

[0011]

[0012] Among them, R1 is One of;

[0015] X is a halogen, and is preferably F, Cl, Br or I; m=4-65, n=0-3, and p is 12, 14 or 16.

[0016] The phosphorus-containing silicon quaternary ammonium salt has only one hydroxyl group in its molecular structure, so the site for reacting with isocyanate is only one end, so that it must be connected to the side chain of polyurethane.

[0017] Preferably, the phosphorus-containing silicon quaternary ammonium salt is prepared by the following steps:

[0018] 53.5-270 parts by weight of organosilicon quaternary ammonium salt, 9-12.5 parts by weight of diisocyanate, and 0.05-0.3 parts by weight of organometallic catalyst are mixed, stirred and reacted at 75°C-85°C for 3-5 hours, and then 11.1 parts by weight of phosphorus-containing diol are added, stirred and reacted at 80°C-90°C for 3-5 hours to obtain phosphorus-containing silicon quaternary ammonium salt.

[0019] The organosilicon quaternary ammonium salt is prepared according to the patent "A kind of organosilicon quaternary ammonium salt modified polyurethane and its preparation method and application" (patent number: ZL 202011559152.7, authorization announcement number: CN112679689 B), and the organosilicon quaternary ammonium salt with an average molecular weight of 1500 to 3500 is preferred.

[0020] More preferably, the diisocyanate is one of toluene diisocyanate (TDI), diphenylmethane-4,4'-diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), p-phenylene diisocyanate (PPDI), xylylene diisocyanate (XDI), 1,4-cyclohexane diisocyanate (CHDI), and naphthalene-1,5-diisocyanate (NDI). More preferably, the diisocyanate is toluene diisocyanate (TDI) or diphenylmethane-4,4'-diisocyanate (MDI).

[0021] More preferably, the organic metal catalyst is at least one of stannous octoate, dibutyltin dilaurate, lead octoate or di-n-butyltin diacetate, and most preferably dibutyltin dilaurate having a good catalytic effect.

[0022] More preferably, the phosphorus-containing diol is preferably a commercial phosphorus-containing diol (trade name FR-D), and its structure is

[0023] The preparation of the phosphorus-containing silicon quaternary ammonium salt is preferably carried out under an inert gas atmosphere.

[0024] Preferably, in the raw material components of the flame retardant antibacterial polyurethane, the molecular weight of the polyether polyol is 200 to 10000, specifically at least one of polyoxypropylene ether polyol (PPG), polytetramethylene ether polyol (PTMEG) or tetramethylene ether copolymer polyol; more preferably, it is polyoxypropylene ether triol with an average molecular weight of 300 to 6000.

[0025] Preferably, in the raw material components of the flame retardant antibacterial polyurethane, the polyester polyol is at least one of adipic acid polyester polyol, pimelic acid polyester polyol, suberic acid polyester polyol, glutaric acid polyester polyol, sebacic acid polyester polyol, oxalic acid polyester polyol, succinic acid polyester polyol, polycaprolactone polyol, polycarbonate polyol, maleic anhydride polyester polyol, phthalic anhydride polyester polyol, para-phenylene polyester polyol or random polyester polyol having an average functionality greater than 2 and an average molecular weight of 400 to 6000; more preferably, it is adipic acid polyester polyol or polycaprolactone polyol having an average functionality equal to 3 and an average molecular weight of 400 to 6000, which is easy to control in the reaction.

[0026] Preferably, in the raw material components of the flame retardant antibacterial polyurethane, the chain extender is at least one of 1,4-butanediol, ethylene glycol, propylene glycol, hexanediol, cyclohexanediol, dihydroxyethyl terephthalate or trimethylolpropane monoallyl ether; more preferably 1,4-butanediol.

[0027] Preferably, in the raw material components of the flame retardant antibacterial polyurethane, the defoaming agent is an organosilicon defoaming agent and / or a mineral oil defoaming agent; more preferably, it is an organosilicon defoaming agent.

[0028] Preferably, in the raw material components of the flame retardant antibacterial polyurethane, the curing agent is one of dimethylthiotoluene diamine (DMTDA, such as Ethacure300), 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA), diethyltoluene diamine (DETDA, such as Ethacure100), 3,5-diamino-4-chlorophenylacetic acid isopropyl ester (such as CuA-60) or 4,4'-methylenebis(2,6-diethyl-3-chloroaniline) (MCDEA); more preferably dimethylthiotoluene diamine (DMTDA, Ethacure300); the organic metal catalyst is at least one of stannous octoate, dibutyltin dilaurate, lead octoate or di-n-butyltin diacetate.

[0029] The preparation method of the flame retardant antibacterial polyurethane comprises the following steps:

[0030] The phosphorus-silicon quaternary ammonium salt, polyether polyol or polyester polyol, diisocyanate and organic metal catalyst are mixed, stirred and reacted at 75-85° C. for 3-5 hours, and then a chain extender, a defoamer and a curing agent are added, and the mixture is cured at 80-90° C. for 10-20 hours to obtain a flame-retardant antibacterial polyurethane.

[0031] The method for preparing the flame retardant antibacterial polyurethane is preferably carried out under an inert gas atmosphere.

[0032] The flame retardant and antibacterial polyurethane prepared by the present invention has excellent flame retardant and antibacterial properties while maintaining the original advantages of polyurethane, and can be widely used in the fields of building materials, car seat cushions, home appliances, fabrics, toys, kitchen utensils, office supplies, food packaging, footwear, medical materials, communication products, etc.

[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0034] (1) The flame retardant and antibacterial polyurethane of the present invention combines the properties of phosphorus-containing flame retardant, organosilicon, quaternary ammonium salt and polyurethane, so that the polyurethane has excellent flame retardant and antibacterial properties while maintaining its original advantages.

[0035] (2) The present invention first prepares a phosphorus-containing silicon quaternary ammonium salt, and then grafts it onto a polyurethane side chain. Since the side chain organosilicon easily migrates to the material surface, the phosphorus-containing flame retardant and quaternary ammonium salt connected thereto are also enriched on the surface, and the phosphorus and silicon flame retardants on the material surface can better prevent the material from burning, and the quaternary ammonium salt on the material surface is more likely to contact with bacteria, thereby improving the antibacterial effect. The phosphorus-containing silicon quaternary ammonium salt contains four flame retardant components, namely phosphorus, silicon, nitrogen and halogen, and can synergistically enhance the flame retardant properties of polyurethane. Among them, phosphorus, silicon and nitrogen are difficult to produce toxic gases when burning, which has little damage to the human body and little pollution to the environment.

[0036] (3) The preparation method of the polyurethane material of the present invention has simple synthesis steps, easy-to-control conditions, safe operation, and cheap and readily available raw materials, which is suitable for industrial production; and no harmful solvents are used, which is environmentally friendly and in line with the development direction of "green materials". DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto. The raw materials involved in the present invention can be purchased directly from the market. For process parameters not specifically specified, conventional techniques can be used. The preparation methods of organosilicon quaternary ammonium salts in the following Examples 1 to 6 correspond one to one to Examples 1 to 6 in the patent "A kind of organosilicon quaternary ammonium salt modified polyurethane and its preparation method and application" (Patent No.: ZL 202011559152.7, Authorization Announcement No.: CN112679689 B).

[0038] The synthesis route of the phosphorus-containing silicon quaternary ammonium salt of the present invention is as follows:

[0039]

[0040] Among them, R1 is One of;

[0043] X is a halogen, and is preferably F, Cl, Br or I; m=4-65, n=0-3, and p is 12, 14 or 16.

[0044] Example 1

[0045] A flame retardant antibacterial polyurethane is prepared by the following steps:

[0046] (1) Preparation of phosphorus-containing silicon quaternary ammonium salt

[0047] 270g of organosilicon quaternary ammonium salt (made from dodecyldimethyl (2-hydroxy)ethylammonium chloride, toluene diisocyanate, and double-terminated hydroxyl polydimethylsiloxane (hydroxyl terminated, with an average molecular weight of 5000)), 9g of toluene diisocyanate, and 0.05g of dibutyltin dilaurate were mixed, stirred and reacted at 75°C for 5h under nitrogen protection, and then 11.1g of phosphorus-containing diol FR-D was added, and stirred and reacted at 80°C for 5h under nitrogen protection to obtain phosphorus-containing silicon quaternary ammonium salt.

[0048] (2) Preparation of flame-retardant and antibacterial polyurethane

[0049] 5 g of phosphorus-containing silicon quaternary ammonium salt, 100 g of polyether triol N330, 18 g of toluene diisocyanate and 0.1 g of dibutyltin dilaurate were mixed, stirred and reacted at 75 ° C for 8 h under nitrogen protection, and then 0.1 g of silicone defoamer and 10 g of dimethylthiotoluene diamine were added. The mixture was cured at 80 ° C for 20 h to obtain a flame retardant antibacterial polyurethane.

[0050] Example 2

[0051] A flame retardant antibacterial polyurethane is prepared by the following steps:

[0052] (1) Preparation of phosphorus-containing silicon quaternary ammonium salt

[0053] 128g of organosilicon quaternary ammonium salt (made from tetradecyldimethyl (2-hydroxy)ethylammonium chloride, diphenylmethane-4,4'-diisocyanate, and double-terminated hydroxyl polydimethylsiloxane (silanol-terminated, with an average molecular weight of 2000)), 12.5g of diphenylmethane-4,4'-diisocyanate, and 0.1g of dibutyltin dilaurate were mixed, stirred and reacted at 80°C for 4h under nitrogen protection, and then 11.1g of phosphorus-containing diol FR-D was added, and stirred and reacted at 85°C for 4h under nitrogen protection to obtain phosphorus-containing silicon quaternary ammonium salt.

[0054] (2) Preparation of flame-retardant and antibacterial polyurethane

[0055] 12g of phosphorus-containing silicon quaternary ammonium salt, 100g of polyoxypropylene ether triol JH-3030, 25.5g of diphenylmethane-4,4'-diisocyanate and 0.1g of dibutyltin dilaurate were mixed, stirred and reacted at 80°C for 6h under nitrogen protection, and then 4g of ethylene glycol, 0.9g of silicone defoamer and 10g of liquid 3,3'-dichloro-4,4'-diaminodiphenylmethane were added and cured at 90°C for 10h to obtain flame-retardant antibacterial polyurethane.

[0056] Example 3

[0057] A flame retardant antibacterial polyurethane is prepared by the following steps:

[0058] (1) Preparation of phosphorus-containing silicon quaternary ammonium salt

[0059] 53.5 g of organosilicon quaternary ammonium salt (made from hexadecyldimethyl (2-hydroxy)ethylammonium chloride, isophorone diisocyanate, and dihydroxy-terminated polydimethylsiloxane (silanol-terminated, with an average molecular weight of 500)), 11.2 g of isophorone diisocyanate, and 0.2 g of lead octylate were mixed, stirred and reacted at 85° C. for 3 h under nitrogen protection, and then 11.1 g of phosphorus-containing diol FR-D was added, and stirred and reacted at 90° C. for 3 h under nitrogen protection to obtain phosphorus-containing silicon quaternary ammonium salt.

[0060] (2) Preparation of flame-retardant and antibacterial polyurethane

[0061] 15g of phosphorus-containing silicon quaternary ammonium salt, 100g of polyoxypropylene ether triol MN-3050, 23g of isophorone diisocyanate and 0.3g of lead octanoate were mixed, stirred and reacted at 90°C for 3 hours under nitrogen protection, 3g of hexanediol and 1.6g of silicone defoamer and 12g of 3,5-diamino-4-chlorophenylacetic acid isopropyl ester were added, and the mixture was cured at 85°C for 15 hours to obtain a flame-retardant antibacterial polyurethane.

[0062] Example 4

[0063] A flame retardant antibacterial polyurethane is prepared by the following steps:

[0064] (1) Preparation of phosphorus-containing silicon quaternary ammonium salt

[0065] 73g of organosilicon quaternary ammonium salt (made from dodecyldimethyl (2-hydroxy)ethylammonium chloride, hexamethylene diisocyanate, and dihydroxy-terminated polydimethylsiloxane (silanol-terminated, with an average molecular weight of 1000)), 9g of hexamethylene diisocyanate, and 0.1g of di-n-butyltin diacetate were mixed, and stirred for reaction at 80°C for 4h under nitrogen protection. Then, 11.1g of phosphorus-containing diol FR-D was added, and stirred for reaction at 85°C for 4h under nitrogen protection to obtain phosphorus-containing silicon quaternary ammonium salt.

[0066] (2) Preparation of flame-retardant and antibacterial polyurethane

[0067] 22g of phosphorus-containing silicon quaternary ammonium salt, 100g of polyoxypropylene ether triol 1618A, 17.5g of hexamethylene diisocyanate and 0.5g of di-n-butyltin diacetate were mixed, stirred and reacted at 75°C for 5h under nitrogen protection, and then 3g of propylene glycol, 1g of silicone defoamer and 3g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline) were added and cured at 80°C for 20h to obtain a flame-retardant antibacterial polyurethane.

[0068] Example 5

[0069] A flame retardant antibacterial polyurethane is prepared by the following steps:

[0070] (1) Preparation of phosphorus-containing silicon quaternary ammonium salt

[0071] 225g of organosilicon quaternary ammonium salt (made from tetradecyl dimethyl (2-hydroxy) ethyl ammonium chloride, toluene diisocyanate, and double-terminated hydroxyl polydimethylsiloxane (silanol-terminated, with an average molecular weight of 4000)), 9g of toluene diisocyanate, and 0.3g of dibutyltin dilaurate were mixed, stirred and reacted at 75°C for 4h under nitrogen protection, and then 11.1g of phosphorus-containing diol FR-D was added, and stirred and reacted at 85°C for 4h under nitrogen protection to obtain phosphorus-containing silicon quaternary ammonium salt.

[0072] (2) Preparation of flame-retardant and antibacterial polyurethane

[0073] 30g of phosphorus-containing silicon quaternary ammonium salt, 100g of polyethylene adipate trimethylolpropane polyol with an average molecular weight of 3000 and a hydroxyl value of 56-60, 18g of toluene diisocyanate and 0.15g of dibutyltin dilaurate were mixed, stirred and reacted at 75°C for 8h under nitrogen protection, and then 3g of dihydroxyethyl terephthalate, 1.2g of mineral oil defoaming agent and 17g of diethyltoluenediamine were added and cured at 80°C for 20h to obtain a flame-retardant antibacterial polyurethane.

[0074] Example 6

[0075] A flame retardant antibacterial polyurethane is prepared by the following steps:

[0076] (1) Preparation of phosphorus-containing silicon quaternary ammonium salt

[0077] 105g of organosilicon quaternary ammonium salt (made from hexadecyldimethyl (2-hydroxy)ethylammonium chloride, diphenylmethane-4,4'-diisocyanate, and double-terminated hydroxyl polydimethylsiloxane (silanol-terminated, with an average molecular weight of 1500)), 12.5g of diphenylmethane-4,4'-diisocyanate, and 0.1g of dibutyltin dilaurate were mixed, stirred and reacted at 85°C for 4h under nitrogen protection, and then 11.1g of phosphorus-containing diol FR-D was added, and stirred and reacted at 90°C for 3h under nitrogen protection to obtain phosphorus-containing silicon quaternary ammonium salt.

[0078] (2) Preparation of flame-retardant and antibacterial polyurethane

[0079] 40g of phosphorus-containing silicon quaternary ammonium salt, 100g of polycaprolactone triol with an average molecular weight of 1500 and a hydroxyl value of 110-116, 30g of diphenylmethane-4,4'-diisocyanate and 0.3g of dibutyltin dilaurate were mixed, stirred and reacted at 85°C for 4h under nitrogen protection, and then 5g of 1,4-butanediol, 2g of mineral oil defoaming agent and 12g of dimethylthiotoluene diamine were added, and the mixture was cured at 85°C for 15h to obtain a flame-retardant antibacterial polyurethane.

[0080] Comparative Example 1

[0081] The preparation of polyurethane containing phosphorus, silicon and quaternary ammonium salt comprises the following steps:

[0082] 0.9 g of phosphorus-containing diol FR-D, 7.9 g of double-terminal hydroxyl polydimethylsiloxane (silanol-terminated, average molecular weight of 2000), 1.3 g of tetradecyl dimethyl (2-hydroxy) ethyl ammonium chloride, 100 g of polyoxypropylene ether triol JH-3030, 25.5 g of diphenylmethane-4,4'-diisocyanate and 0.1 g of dibutyltin dilaurate were mixed, stirred and reacted at 80°C for 6 h under nitrogen protection, and then 4 g of ethylene glycol and 0.9 g of silicone defoamer and 10 g of liquid 3,3'-dichloro-4,4'-diaminodiphenylmethane were added, and the mixture was cured at 90°C for 10 h to obtain a quaternary ammonium salt-modified polyurethane.

[0083] Comparative Example 2

[0084] The preparation of polyurethane containing phosphorus, silicon and quaternary ammonium salt comprises the following steps:

[0085] 2.2g of phosphorus-containing diol FR-D, 4.9g of double-terminal hydroxyl polydimethylsiloxane (silanol-terminated, average molecular weight of 500), 3.5g of hexadecyldimethyl (2-hydroxy)ethylammonium chloride, 100g of polyoxypropylene ether triol MN-3050, 23g of isophorone diisocyanate and 0.3g of lead octanoate were mixed, stirred and reacted at 90°C for 3 hours under nitrogen protection, 3g of hexanediol and 1.6g of silicone defoamer and 12g of 3,5-diamino-4-chlorophenylacetic acid isopropyl were added, and the mixture was cured at 85°C for 15h to obtain a quaternary ammonium salt modified polyurethane.

[0086] Comparative Example 3

[0087] The preparation of polyurethane containing phosphorus, silicon and quaternary ammonium salt comprises the following steps:

[0088] 2.6g of phosphorus-containing diol FR-D, 11.9g of double-terminal hydroxyl polydimethylsiloxane (silanol-terminated, average molecular weight of 1000), 3.5g of dodecyldimethyl (2-hydroxy) ethyl ammonium chloride, 100g of polyoxypropylene ether triol 1618A, 17.5g of hexamethylene diisocyanate and 0.5g of di-n-butyltin diacetate were mixed, stirred and reacted at 75°C for 5h under nitrogen protection, and then 3g of propylene glycol and 1g of silicone defoamer and 3g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline) were added, and the mixture was cured at 80°C for 20h to obtain a quaternary ammonium salt-modified polyurethane.

[0089] Comparative Example 4

[0090] The preparation of polyurethane containing phosphorus, silicon and quaternary ammonium salt comprises the following steps:

[0091] 1.4g of phosphorus-containing diol FR-D, 24.5g of double-terminal hydroxyl polydimethylsiloxane (silanol-terminated, average molecular weight of 4000), 2.0g of tetradecyl dimethyl (2-hydroxy) ethyl ammonium chloride, 100g of polyethylene adipate trimethylolpropane ester polyol with an average molecular weight of 3000 and a hydroxyl value of 56-60, 25g of toluene diisocyanate and 0.15g of dibutyltin dilaurate were mixed, stirred and reacted at 75°C for 8h under nitrogen protection, and then 3g of dihydroxyethyl terephthalate, 1.2g of mineral oil defoamer and 17g of diethyltoluenediamine were added, and the mixture was cured at 80°C for 20h to obtain a quaternary ammonium salt modified polyurethane.

[0092] The polyurethanes prepared in the above examples and comparative examples were subjected to oxygen index test and antibacterial property test. The results are shown in Table 1.

[0093] Table 1 Oxygen index and antibacterial rate of polyurethane

[0094] sample Limiting oxygen index (%) Staphylococcus aureus inhibition rate (%) Escherichia coli inhibition rate (%) Example 1 21.1 37.8 34.3 Example 2 22.5 71.5 70.1 Example 3 25.2 88.2 87.0 Example 4 27.8 93.2 92.4 Example 5 28.6 92.5 90.8 Example 6 31.8 94.8 93.6 Comparative Example 1 21.2 70.2 68.5 Comparative Example 2 23.5 85.5 84.2 Comparative Example 3 25.2 88.2 87.3 Comparative Example 4 26.4 86.5 86.1

[0095] It can be seen from Table 1 that Examples 1-6 are flame-retardant and antibacterial polyurethanes, and their flame retardancy and antibacterial properties are enhanced as the content of phosphorus-containing silicon quaternary ammonium salt increases.

[0096] Comparative Examples 1-4 are phosphorus-containing, silicon-containing, quaternary ammonium salt polyurethanes, and phosphorus-containing diols, organosilicon, and quaternary ammonium salts do not form a molecule and are added to the reaction system respectively. Embodiments 2, 3, 4, and 5 are successively the same in type and content as the phosphorus-containing diols, organosilicon, and quaternary ammonium salts in Comparative Examples 1, 2, 3, and 4. By comparison, it can be seen that the flame retardancy and antibacterial properties of Embodiments 2, 3, 4, and 5 are stronger than those of the corresponding Comparative Examples 1, 2, 3, and 4, indicating that organosilicon can help phosphorus-containing groups and quaternary ammonium salt groups migrate to the material surface, improving flame retardancy and sterilization efficiency.

[0097] The above embodiments illustrate that the introduction of phosphorus-containing silicon quaternary ammonium salt into polyurethane can make the polyurethane have excellent flame retardancy and antibacterial properties, especially the phosphorus-containing silicon quaternary ammonium salt of the present invention connected to the side chain can enhance this advantage.

[0098] The performance testing methods in the above embodiments and comparative examples are as follows:

[0099] The oxygen index was measured using a JF-3 oxygen index tester (Analytical Instrument, Jiangning District, Nanjing) according to GB / T 2406-1993, with a sample size of 120 mm × 10 mm × 4 mm.

[0100] Antibacterial experiment: The test bacteria were Escherichia coli (ATCC 8739) and Staphylococcus aureus (ATCC 6538P). They were cultured in nutrient broth at 37°C for 24 hours to obtain the mother solution. 0.2 mL of the mother solution was taken out with a pipette and added to a test tube containing 1.8 mL of sterile water. The bacterial solution was then diluted 10 times several times. The bacterial content was selected to be 1×10 5 ~5×10 5 CFU / mL of bacterial solution is used as the inoculated sample bacterial solution. According to the national standard GB / T4789.2-2010, take 0.4mL of the inoculated bacterial solution and evenly add it to the control group and the antibacterial material group, and cover the sample with a polyethylene film. Put it in a blank culture dish, place it in a clean bench with natural light, and culture it at 37°C for 6 hours. Wash the sample and polyethylene film that have been cultured for 6 hours with 10mL of sterile water several times, and collect the washed liquid. Take out 0.2mL of the liquid and spread it on the solid agar medium, and culture it in a constant temperature and humidity chamber at 37°C for 24 hours. Count the plaques on the sample and calculate the antibacterial rate. Do 3 groups in parallel and take the average value.

[0101] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A flame retardant and antibacterial polyurethane, characterized in that: The raw materials for preparing the flame-retardant antibacterial polyurethane include: 5 to 40 parts by weight of phosphorus-containing silicon quaternary ammonium salt, 100 parts by weight of polyether polyol or polyester polyol, 17.5 to 30 parts by weight of diisocyanate, 0.1 to 0.5 parts by weight of organic metal catalyst, 0 to 5 parts by weight of chain extender, 0.1 to 2.0 parts by weight of defoamer and 3 to 17 parts by weight of curing agent.

2. The flame retardant and antibacterial polyurethane according to claim 1, characterized in that: The phosphorus-containing silicon quaternary ammonium salt is prepared by the following steps: 53.5 to 270 parts by weight of an organic silicon quaternary ammonium salt, 9 to 12.5 parts by weight of a diisocyanate, and 0.05 to 0.3 parts by weight of an organic metal catalyst are mixed, and the mixture is stirred and reacted at 75° C. to 85° C. for 3 to 5 hours, and then 11.1 parts by weight of a phosphorus-containing diol is added, and the mixture is stirred and reacted at 80° C. to 90° C. for 3 to 5 hours to obtain the phosphorus-containing silicon quaternary ammonium salt.

3. The flame retardant and antibacterial polyurethane according to claim 2, characterized in that: The average molecular weight of the organosilicon quaternary ammonium salt is 1500 to 3500; The diisocyanate is one of toluene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, p-phenylene diisocyanate, xylylene diisocyanate, 1,4-cyclohexane diisocyanate, and naphthalene-1,5-diisocyanate; The organic metal catalyst is at least one of stannous octoate, dibutyltin dilaurate, lead octoate or di-n-butyltin diacetate; The phosphorus-containing diol is a commercial phosphorus-containing diol, and its structure is 4. The flame retardant and antibacterial polyurethane according to claim 1, characterized in that: The polyether polyol has a molecular weight of 200 to 10,000 and is at least one of polyoxypropylene ether polyol, polytetramethylene ether polyol or tetramethylene ether polyol.

5. The flame retardant and antibacterial polyurethane according to claim 1, characterized in that: The polyester polyol is at least one of adipic acid polyester polyol, pimelic acid polyester polyol, suberic acid polyester polyol, glutaric acid polyester polyol, sebacic acid polyester polyol, oxalic acid polyester polyol, succinic acid polyester polyol, polycaprolactone polyol, polycarbonate polyol, maleic anhydride polyester polyol, phthalic anhydride polyester polyol, para-phenylene polyester polyol or random polyester polyol having an average functionality greater than 2 and an average molecular weight of 400 to 6000.

6. The flame retardant and antibacterial polyurethane according to claim 1, characterized in that: The polyether polyol is a polyoxypropylene ether triol with an average molecular weight of 300 to 6000; the polyester polyol is adipic acid polyester polyol or polycaprolactone polyol with an average functionality of 3 and an average molecular weight of 400 to 6000.

7. The flame retardant and antibacterial polyurethane according to claim 1, characterized in that: The chain extender is at least one of 1,4-butanediol, ethylene glycol, propylene glycol, hexanediol, cyclohexanediol, dihydroxyethyl terephthalate or trimethylolpropane monoallyl ether; The defoamer is a silicone defoamer and / or a mineral oil defoamer; The curing agent is one of dimethylthiotoluenediamine, 3,3'-dichloro-4,4'-diaminodiphenylmethane, diethyltoluenediamine, 3,5-diamino-4-chlorophenylacetic acid isopropyl ester or 4,4'-methylenebis(2,6-diethyl-3-chloroaniline); The organic metal catalyst is at least one of stannous octoate, dibutyltin dilaurate, lead octoate or di-n-butyltin diacetate.

8. The method for preparing the flame retardant antibacterial polyurethane according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing phosphorus-silicon quaternary ammonium salt, polyether polyol or polyester polyol, diisocyanate and an organic metal catalyst, stirring and reacting at 75-85° C. for 3-5 hours, adding a chain extender, a defoamer and a curing agent, and curing at 80-90° C. for 10-20 hours to obtain a flame-retardant antibacterial polyurethane.

9. The preparation method according to claim 8, characterized in that: The preparation method is carried out under an inert gas atmosphere.

10. Use of the flame-retardant antibacterial polyurethane according to any one of claims 1 to 7 in the fields of building materials, vehicle seat cushions, household appliances, fabrics, toys, kitchen utensils, office supplies, food packaging, footwear, medical materials and communication products.

Citation Information

Patent Citations

  • A silicone quaternary ammonium salt modified polyurethane, its preparation method and application

    CN112679689B