High-flame-retardant low-VOC (volatile organic compound) polyurethane light foam composition as well as preparation method and application thereof
By combining polyether polyols, isocyanates and shrimp shell treatment materials, high flame retardant and low VOC polyurethane light foam was prepared, which solved the problems of poor flame retardant performance and high VOC of automotive polyurethane porous materials, and achieved density, Optimization of compression strength and flame retardant performance, suitable for bus roof applications.
Patent Information
- Application Number
- CN202411246116.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, polyurethane porous materials for automotive use have poor flame retardant properties and high VOC, and cannot be used to form a foam first and then perform ceiling molding, which poses inconvenience in construction and risk of environmental pollution.
Compositions of components A, B, C are used, wherein component A includes polyether polyol, polyethylene glycol, foam stabilizer and catalyst, component B is isocyanate and flame retardant polyester, and component C is shrimp and crab The shell treatment substance is prepared by a specific weight ratio and treatment method to prepare a high flame retardant and low VOC polyurethane light foam, combined with aromatic isocyanate self-polytic, flame retardant polyester prepolymerization and high molecular weight phosphate liquid flame retardant, forming a Composition with good flame retardant properties and low VOC.
The density between 12.1 and 18.3 kg/m3 was optimized, compression strength and elongation of breaking, and the flame retardant performance was improved to 28.5 and 31.5%, reducing VOC, and meeting the application of high flame retardant and low VOC polyurethane light foam. Needs, especially suitable for bus roofs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a highly flame-retardant, low-VOC polyurethane lightweight foam composition, a preparation method and an application thereof. Background Art
[0002] According to statistics from the World Automobile Manufacturers Association, the global automobile production is generally stable and shows an increasing trend year by year. The three major issues of energy, environmental protection and safety have also become the focus of major automobile manufacturers. Seeking lightweight materials for use on the car body can greatly reduce the weight of the car body and reduce energy consumption. Polyurethane full water low-density spraying is often carried out in this spraying process because of its advantages such as convenient construction, low density, sound absorption and noise reduction. However, the spraying process is prone to produce fine foam particles, which can easily cause harm to the life and health of the constructors. In addition, there are certain risks and inconveniences in spraying construction in the limited space of the bus. If the ceiling can be formed in a similar way to a car and then fixed on the roof, both the construction environment and the interior environment will be greatly improved. In addition, according to China's new transportation industry standard JT-1095, the fire resistance of commercial bus insulation foam is stipulated, and the oxygen index required for the foam is much higher than before.
[0003] Highly flame-retardant foams, such as those with an oxygen index greater than 26%, are basically sprayed with rigid foam. Spray coatings generally have a high VOC content, and the spraying construction process will cause environmental pollution and physical harm to construction workers. Low-density spray coatings cannot be foamed first and then sliced and formed for use on car roofs. Existing lightweight foams are mostly used for sound-absorbing parts such as the front and engine hood of cars. The requirements for flame retardancy are not high. The flame retardancy is at the A0 level, and horizontal combustion is less than 100mm / s. There is currently no density of 12 to 18kg / m 3 The oxygen index of the lightweight foam can reach the requirement of more than 28.2%. Therefore, it is very necessary to develop a highly flame-retardant and low-VOC polyurethane lightweight foam for the roof.
[0004] CN108148168A provides a method for preparing highly flame-retardant, low-density polyurethane foam, which has the beneficial effect of preparing polyurethane foam with a density range of 5.5 to 9 kg / m in an environmentally friendly and pollution-free manner. 3 The oxygen index range is 22% to 26% for the passenger car ceiling with all-water low-density flame-retardant polyurethane spray foam. However, it can only be sprayed, and it is impossible to foam first and then form the ceiling, and the oxygen index is <28.2%.
[0005] CN110982030A discloses a one-step continuous production method for preparing lightweight polyurethane semi-rigid foam. The formula contains a combined polyether, a combined isocyanate, and related additives. The combined polyether ratio is as follows by mass: polyether polyol composition: 80-90 parts; flame retardant: 10-20 parts; cell opener: 2-10 parts; chain extender: 5-10 parts. The foam produced by this method has the advantages of low density and finer pores, but uses phosphate flame retardants, which are volatile and have a strong odor, and do not meet the environmental protection requirements for the development of automotive interiors. In addition, the content does not mention the flame retardant properties of the foam.
[0006] CN116874721A adopts a low-density porous material, which is composed of components A, B, C and D. In terms of weight ratio, A:B:C:D=100:85-250:0.5-10:10-55; component A, in terms of weight ratio, comprises: 20-60 parts of polyether polyol A, 20-50 parts of polyether polyol B, 0.5-11 parts of open-cell polyether polyol, 0.2-2.5 parts of foam stabilizer, and 3-18 parts of water; component B is isocyanate; component C is a combination of a small molecule compound and a catalyst; component D is a combination of an intumescent flame retardant material and a porous nano material in a weight ratio of 1:1-10; the expansion ratio of the intumescent flame retardant material is greater than 50; the particle size of the porous nano material is ≥3000 mesh, and the specific surface area is greater than 10000cm 2 / g and the technical solution for its preparation have effectively solved the problems of high density, poor sound absorption and poor flame retardancy of automotive polyurethane porous materials existing in the prior art, but its flame retardancy is not high, only meeting the A0 level and failing to meet the requirement of oxygen index ≥ 28.2%. Summary of the invention
[0007] One of the technical problems to be solved by the present invention is the poor flame retardancy and high VOC of the prior art polyurethane porous material for automobiles, and a composition of highly flame retardant and low VOC polyurethane lightweight foam is provided, which has the advantages of good flame retardancy and low VOC.
[0008] The second technical problem to be solved by the present invention is to provide a method for preparing a highly flame-retardant, low-VOC polyurethane lightweight foam corresponding to the first technical problem to be solved.
[0009] The third technical problem to be solved by the present invention is to provide an application of a highly flame-retardant, low-VOC polyurethane lightweight foam corresponding to the first technical problem to be solved.
[0010] To solve one of the above technical problems, the technical solution provided by the present invention is as follows: a composition of highly flame-retardant, low-VOC polyurethane lightweight foam, comprising: a component A, a component B and a component C, wherein the weight ratio of component A, component B and component C is 50:68-115:7.5-20, wherein component A comprises the following components in weight: 50-70 parts of polyether polyol I, 20-30 parts of polyether polyol II, 10-20 parts of polyethylene glycol, 2-5.5 parts of foam stabilizer, 0.6-0.85 parts of combined catalyst, 10-20 parts of liquid flame retardant, and 8-15 parts of water; component B is a composition of isocyanate and flame-retardant polyester in a weight ratio of 10:1-1.5; component C is 25-40 parts of shrimp and crab shell treated material. The polyether polyol I is polymerized from ethylene oxide and propylene oxide with glycerol as the initiator, with a functionality of 3, a molecular weight of 4000-6000, and a hydroxyl value of 25-45 mgKOH / g; the polyether polyol II is polymerized from propylene oxide with glycerol and sorbitol as the mixed initiators, with a functionality of 3-6, a molecular weight of 300-400, and a hydroxyl value of 400-500 mgKOH / g; the polyethylene glycol is a condensation product of ethylene oxide and water, with a functionality of 2, a molecular weight of 300-500, and a hydroxyl value of 250-300 mgKOH / g; the component B is prepolymerized from isocyanate and flame-retardant polyester, with an isocyanate group content of 25-28%; the shrimp and crab shell treated material of the component C is a shrimp or crab shell that is dried, crushed, and then soaked in alkali solution to obtain a shrimp and crab shell treated material, which has certain flame retardant properties.
[0011] In the above technical solution, the polyethylene glycol in component A is at least one of PEG-400 and PEG-350, and has been dehydrated to have a water content of ≤0.01wt%, and has good stability and compatibility.
[0012] In the above technical scheme, the combined catalyst in component A is composed of catalyst I and catalyst II, and the weight ratio of the two is 6 to 8:1. Catalyst I is selected from at least one of A1, ZF-10, and NE-300, and catalyst II is a trimerization catalyst selected from at least one of PC46, PC41, and TMR-2.
[0013] In the above technical solution, the liquid flame retardant is a high molecular weight phosphate ester, selected from at least one of Antiblaze V66, Antiblaze V500, and Antiblaze V610.
[0014] In the above technical solution, the foam stabilizer is selected from at least one of B8715, B8002, L580, and L668.
[0015] In the above technical scheme, the isocyanate in component B is selected from at least one of pure MDI, crude MDI, PM200, M20S, 5005, carbonized diamine-modified MDI, MDI-50 or TDI, and the flame-retardant polyester is selected from at least one of PS-2132, HF-8734 and PS-2412.
[0016] In order to solve the second of the above technical problems, the technical solution adopted by the present invention is as follows: A method for preparing highly flame-retardant and low-VOC polyurethane lightweight foam comprises the following steps:
[0017] (1) preparing component A: adding 50-70 parts of polyether polyol I, 20-30 parts of polyether polyol II, 10-20 parts of polyethylene glycol, 2-5.5 parts of foam stabilizer, 0.6-0.85 parts of combined catalyst, and 10-20 parts of liquid flame retardant in a container in order by weight, and stirring the components thoroughly;
[0018] (2) Preparation of component B: adding isocyanate to a reaction kettle, stirring and evacuating, controlling the temperature at 60-80° C., and after nitrogen replacement, adding flame-retardant polyester dropwise, the weight ratio of isocyanate to flame-retardant polyester is 10:1-1.5, and the reaction time is about 180 min;
[0019] (3) preparing component C: drying shrimp shells or crab shells and then crushing them, soaking the obtained shrimp shells or crab shells in alkali solution for about 24 hours, filtering and separating the precipitate to obtain the shrimp shell processed material;
[0020] (4) Control the ambient temperature to 19-22° C., add component C to component B and mix quickly, then add component A and stir quickly for 15-25 seconds. After stirring evenly, immediately pour into a foaming box for foaming to obtain the product.
[0021] In order to solve the third of the above technical problems, the technical solution adopted by the present invention is as follows: application of a composition of highly flame-retardant and low-VOC polyurethane lightweight foam in the roof of a bus.
[0022] By adopting the technical scheme of the present invention, a composition of highly flame-retardant and low-VOC polyurethane lightweight foam can be prepared, and the advantages of the technical scheme are as follows: first, by adopting a trimerization catalyst, aromatic isocyanate can be self-polymerized into a trimer to form an isocyanate ring, which has good heat resistance, good flame penetration resistance, and low combustion smoke; second, the flame-retardant polyester and isocyanate are prepolymerized, which can form a large number of benzene ring structures on the one hand, and also introduce a large number of flame-retardant nitrogen elements, which can greatly improve the flame retardant performance; on the other hand, the flame-retardant polyester and isocyanate are prepolymerized to form a prepolymer, which can avoid the polyester Hydrolysis in the composition; third, the liquid flame retardant adopts high molecular weight phosphate esters, which have long molecular chains and contain a large amount of nitrogen and phosphorus elements, and have the characteristics of good flame retardancy, low volatility and low VOC; fourth, shrimp and crab shell processing materials are used as solid flame retardants. First, they can form a glassy or stable foam covering layer at high temperature to isolate oxygen, and some of the proteins inside can form a carbonized layer to prevent further thermal decomposition of the polymer; secondly, shrimp and crab shells contain a certain amount of chitosan, which has a certain flame retardancy. Finally, shrimp and crab shells are rich renewable biological resources, which are both green and environmentally friendly and cheap and easy to obtain. The prepared composite material of a highly flame-retardant, low-VOC polyurethane lightweight foam has a density (12.1~18.3kg / m 3 ), compressive strength (8.4 ~ 20.6KPa) and elongation at break (12.5 ~ 25.6%) can meet the use conditions, and it has the advantages of good flame retardant properties (28.5 ~ 31.5%, the higher the LOI, the better the flame retardant properties) and low VOC, and has achieved good technical effects. DETAILED DESCRIPTION
[0023] The present invention is further described below in conjunction with specific embodiments. The described embodiments are only a part of the embodiments of the present invention, but not all of the embodiments.
[0024] Table 1 List of raw materials
[0025]
[0026]
[0027] Example 1
[0028] (1) Preparation of component A: In a container, add 60 parts of polyether polyol I, 25 parts of polyether polyol II, 10 parts of polyethylene glycol, 2.5 parts of foam stabilizer B8715, 1.0 parts of foam stabilizer B8002, 0.6 parts of catalyst I: NE-300, 0.08 parts of catalyst II: PC46, 10 parts of liquid flame retardant Antiblaze V610, and 11 parts of water in order by weight, and stir the components thoroughly;
[0029] (2) Preparation of component B: 200 parts of isocyanate were added to a reaction kettle, stirred and evacuated, the temperature was controlled at 60-80° C., after nitrogen replacement, 20 parts of flame-retardant polyester were added dropwise, and the reaction was carried out for about 180 minutes;
[0030] (3) preparing component C: drying shrimp shells or crab shells and then crushing them, soaking the obtained shrimp shells or crab shells in alkali solution for about 24 hours, filtering and separating the precipitate to obtain the shrimp shell processed material;
[0031] (4) Control the ambient temperature to 19-22° C., add component C to component B and mix quickly, then add component A and stir quickly for 15-25 seconds. After stirring evenly, immediately pour into a foaming box for foaming to obtain the product.
[0032] Embodiments 2 to 8
[0033] Examples 2 to 8 are carried out according to the steps in Example 1, except that the reaction raw materials and raw material ratios in the foaming formula are different, as shown in Table 2; the performance index data of the obtained highly flame-retardant, low-VOC polyurethane lightweight foam are shown in Tables 4 and 5.
[0034] Table 2 Weight percentage of each component in the foaming formula of highly flame-retardant low-VOC polyurethane lightweight foam in Examples 1 to 8
[0035]
[0036]
[0037] Comparative Examples 1 to 4
[0038] (1) Prepare the raw materials according to the weight proportions of the components in Table 3;
[0039] (2) Preparation of component A: Add the weighed components in the container in order according to the weight proportions in step (1), stir for 15 seconds, the material temperature is 20° C., and mix thoroughly;
[0040] (3) Controlling the ambient temperature to 20°C, quickly mixing component A and component B, and immediately pouring them into a foaming box for foaming after stirring evenly, to obtain a polyurethane lightweight foam material, the performance index data of which are shown in Table 4.
[0041] Table 3 Weight percentage of each component in the foaming formula of polyurethane high flame retardant low VOC polyurethane lightweight foam of Comparative Examples 1 to 4
[0042]
[0043] Table 4 Performance test data of highly flame-retardant low VOC polyurethane lightweight foams of Examples 1 to 8 and Comparative Examples 1 to 4
[0044]
[0045] Note: ND means not detected (less than the detection limit of the method).
[0046] The test method for the performance in Table 4 is as follows:
[0047] Density: Tested in accordance with GB / T 6343-2009;
[0048] Compression strength: tested in accordance with GB / T 8813-2020;
[0049] Elongation at break: Tested in accordance with GB / T 6344-2008;
[0050] LOI (%): Tested according to GB / T 2406.2, required to be ≥28.2%;
[0051] Benzene: Tested according to Q / ZK JS408-202005;
[0052] Toluene: Tested according to Q / ZK JS408-202005;
[0053] Ethylbenzene: Tested according to Q / ZK JS408-202005;
[0054] Xylene: Tested according to Q / ZK JS408-202005;
[0055] Styrene: Tested according to Q / ZKJS408-202005;
[0056] Formaldehyde: Tested according to Q / ZK JS336-202104, required to be ≤20mg / kg.
[0057] As shown in Table 4, the highly flame-retardant and low-VOC polyurethane lightweight foams prepared in Examples 1 to 8 of the present invention have a density (12.1 to 18.3 kg / m 3 ), compressive strength (8.4 ~ 20.6KPa) and elongation at break (12.5 ~ 25.6%) all meet the requirements, it not only has good flame retardant properties (28.5 ~ 31.5%), but also greatly reduces the VOC of the product, which can meet the application in bus roofs.
Claims
1. A composition of highly flame-retardant, low-VOC polyurethane lightweight foam, comprising: The invention is composed of component A, component B and component C, wherein the weight ratio of component A, component B and component C is 50:68-115:7.5-20, wherein component A comprises the following components by weight: 50-70 parts of polyether polyol I, 20-30 parts of polyether polyol II, 10-20 parts of polyethylene glycol, 2-5.5 parts of foam stabilizer, 0.6-0.85 parts of combined catalyst, 10-20 parts of liquid flame retardant and 8-15 parts of water; component B is a composition of isocyanate and flame retardant polyester in a weight ratio of 10:1-1.5; component C is 25-40 parts of shrimp and crab shell treated material; the polyether polyol I is prepared by polymerization of ethylene oxide and propylene oxide with glycerol as the initiator, and has a functionality of 3. The molecular weight is 4000-6000, and the hydroxyl value is 25-45 mgKOH / g; the polyether polyol II is prepared by polymerization of propylene oxide with glycerol and sorbitol as mixed initiators, with a functionality of 3-6, a molecular weight of 300-400, and a hydroxyl value of 400-500 mgKOH / g; the polyethylene glycol is a condensation product of ethylene oxide and water, with a functionality of 2, a molecular weight of 300-500, and a hydroxyl value of 250-300 mgKOH / g; the component B is prepared by prepolymerization of isocyanate and flame-retardant polyester, and the isocyanate content is 25-28%; the shrimp and crab shell treated material of the component C is a shrimp or crab shell that is dried, crushed, and then soaked in alkali solution to obtain a shrimp and crab shell treated material, which has certain flame retardant properties.
2. The highly flame-retardant, low-VOC polyurethane lightweight foam composition according to claim 1, characterized in that: The polyethylene glycol in component A is at least one of PEG-400 and PEG-350, and has been dehydrated to have a water content of ≤0.01 wt %, and has good stability and compatibility.
3. The highly flame-retardant, low-VOC polyurethane lightweight foam composition according to claim 1, characterized in that: The combined catalyst in component A is composed of catalyst I and catalyst II, the weight ratio of which is 6 to 8:
1. Catalyst I is selected from at least one of A1, ZF-10, and NE-300, and catalyst II is a trimerization catalyst selected from at least one of PC46, PC41, and TMR-2.
4. The highly flame-retardant, low-VOC polyurethane lightweight foam composition according to claim 1, characterized in that: The liquid flame retardant is a high molecular weight phosphate ester, selected from at least one of Antiblaze V66, Antiblaze V500 and Antiblaze V610.
5. The highly flame-retardant, low-VOC polyurethane lightweight foam composition according to claim 1, characterized in that: The foam stabilizer is selected from at least one of B8715, B8002, L580 and L668.
6. The highly flame-retardant, low-VOC polyurethane lightweight foam composition according to claim 1, characterized in that: The isocyanate in component B is selected from at least one of pure MDI, crude MDI, PM200, M20S, 5005, carbonized diamine-modified MDI, MDI-50 or TDI, and the flame-retardant polyester is selected from at least one of PS-2132, HF-8734 and PS-2412.
7. The method for preparing the highly flame-retardant, low-VOC polyurethane lightweight foam composition according to claim 1 comprises the following steps: (1) preparing component A: adding 50-70 parts of polyether polyol I, 20-30 parts of polyether polyol II, 10-20 parts of polyethylene glycol, 2-5.5 parts of foam stabilizer, 0.6-0.85 parts of combined catalyst, and 10-20 parts of liquid flame retardant in a container in order by weight, and stirring the components thoroughly; (2) Preparation of component B: adding isocyanate to a reaction kettle, stirring and evacuating, controlling the temperature at 60-80° C., and after nitrogen replacement, adding flame-retardant polyester dropwise, the weight ratio of isocyanate to flame-retardant polyester is 10:1-1.5, and the reaction time is about 160-200 min; (3) preparing component C: drying shrimp shells or crab shells and then crushing them, soaking the obtained shrimp shells or crab shells in alkali solution for about 24 hours, filtering and separating the precipitate to obtain the shrimp shell processed material; (4) Control the ambient temperature to 19-22° C., add component C to component B and mix quickly, then add component A and stir quickly for 15-25 seconds. After stirring evenly, immediately pour into a foaming box for foaming to obtain the product.
8. Use of the highly flame-retardant, low-VOC polyurethane lightweight foam composition of claim 1 in a passenger car roof.