Perfluoropolyether silane compound as well as preparation method and application thereof
By reacting the silane coupling agent with the perfluoropolyether compound, forming the perfluoropolyether silane compound and grafting it onto the perfluoropolyether main chain, the adhesion and wear resistance of the perfluoropolyether compound to the substrate are solved. The poor problem has achieved high adhesion and wear resistance on glass substrates, and is suitable for anti-fingerprint oil and surface treatment of touch screen equipment.
Patent Information
- Application Number
- CN202411270727.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing perfluoropolyether compounds have little adhesion to the substrate and poor wear resistance, making it difficult to meet the needs of anti-fingerprint oil and wear resistance during long-term use of touch screen equipment.
By reacting the silane coupling agent with the perfluoropolyether compound, a perfluoropolyether silane compound is formed and directly grafted onto the perfluoropolyether backbone through amide bonds, ester bonds or imine bonds, it is enhanced on the glass base Adhesion and wear resistance on the material.
It has achieved good adhesion and wear resistance of perfluoropolyether silane compounds on glass substrates, and has excellent hydrophobicity and oleophobicity. It is suitable for anti-fingerprint oil, coatings and surface treatment agents. It has simple operation and product collection. High rate.
Smart Images

Figure CN119081099A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a perfluoropolyether silane compound and a preparation method and application thereof. Background Art
[0002] Nowadays, electronic devices are increasingly used in our daily lives, and there are more and more touch-screen devices. However, during long-term use, the sliding of fingers can easily cause water and oil stains. Therefore, high requirements are placed on the hydrophobic and oleophobic effects and wear resistance of touch-screen materials.
[0003] At present, perfluoropolyether materials have important applications in the field of anti-fingerprint oil. Coating perfluoropolyether materials on substrates can reduce the surface energy of the substrate and improve its hydrophobic and oleophobic properties. However, the adhesion of perfluoropolyether alone to the substrate is very small and its wear resistance is very poor. Summary of the invention
[0004] In order to overcome the technical defects of the prior art such as the weak adhesion between the perfluoropolyether compound and the substrate and the poor wear resistance, the present invention provides a perfluoropolyether silane compound and a preparation method and application thereof. The perfluoropolyether silane compound of the present invention has good adhesion and wear resistance on the glass substrate.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a perfluoropolyether silane compound, the structure of which is as follows:
[0007]
[0008] Wherein, M' is methylene, M" is
[0009] Alternatively, M' is carbonyl, M" is -O- or
[0010] X', X" are each independently hydrogen, phenyl or the following groups:
[0011]
[0012] Y is a C1-C8 alkylene group, a C1-C8 heteroalkylene group, a C1-C8 alkylene group substituted with a substituent, or a C1-C8 heteroalkylene group substituted with a substituent; the heteroatom of the C1-C8 heteroalkylene group is O or N, and the number of heteroatoms is 1-2; the substituent is an epoxy group, a methacryloyloxy group, a phenyl group, an amino group or a halogen atom;
[0013] Z" is a chemical bond, a phenylene group or an imino group;
[0014] R', R", R'" are each independently a C1-C4 alkyl group;
[0015] X' and X" are not hydrogen or phenyl at the same time;
[0016] The average value of n is 6-100.
[0017] In the present invention, the average value of n may be 10-20, such as 16.1-18.0.
[0018] In the present invention, Y is preferably a C1-C8 alkylene group, such as a C3 alkylene group.
[0019] In the present invention, the mass content of fluorine element in the perfluoropolyether silane compound can be 50%-70%.
[0020] In certain embodiments of the present invention, M' is a carbonyl group, M" is X" is phenyl.
[0021] In certain embodiments of the present invention, M' is methylene and M" is -NH-.
[0022] In certain embodiments of the present invention, M' is carbonyl and M" is -O-.
[0023] In certain specific embodiments of the present invention, Z" is a chemical bond, Y is a C1-C8 alkylene group, and the C1-C8 alkylene group is a C3 alkylene group, such as a C3 straight-chain alkylene group.
[0024] In certain specific embodiments of the present invention, the C1-C8 heteroalkylene group is
[0025]
[0026] In certain specific embodiments of the present invention, the epoxy group is an ethylene oxide group or a propylene oxide group.
[0027] In certain embodiments of the present invention, R', R", and R'" are each independently methyl or ethyl.
[0028] In one specific embodiment of the present invention, the structural formula of the perfluoropolyether silane compound is as follows:
[0029]
[0030] Among them, the average value of n is 16.1.
[0031] In one specific embodiment of the present invention, the structural formula of the perfluoropolyether silane compound is as follows:
[0032]
[0033] Among them, the average value of n is 16.1.
[0034] In one specific embodiment of the present invention, the structural formula of the perfluoropolyether silane compound is as follows:
[0035]
[0036] Among them, the average value of n is 16.1.
[0037] In a second aspect, the present invention provides a method for preparing the perfluoropolyether silane compound as described above, comprising the following steps: reacting a K-type perfluoropolyether compound and a silane coupling agent in a first solvent.
[0038] In the present invention, the K-type perfluoropolyether compound can be selected from one or more of K-type perfluoropolyether alcohol, K-type perfluoropolyether acyl chloride, K-type perfluoropolyether acyl fluoride and K-type perfluoropolyether methyl ester.
[0039] In the present invention, the weight average molecular weight of the K-type perfluoropolyether compound may be 1000-15000 g / mol, for example 2972 or 3000 g / mol.
[0040] In the present invention, the silane coupling agent can be selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, 3-phenylaminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane.
[0041] In the present invention, the molar ratio of the K-type perfluoropolyether compound to the silane coupling agent may be 1:(0.9-1.2), for example, 15.00:14.88, 10.00:11.16 or 10.00:11.29.
[0042] In the present invention, the first solvent may be tetrahydrofuran or a fluorocarbon solvent.
[0043] In the present invention, the usage ratio of the K-type perfluoropolyether compound to the first solvent may be 10.00 mmol:(150-200) g.
[0044] In the present invention, the reaction temperature may be 30-80°C, for example 30°C.
[0045] In the present invention, the reaction time may be 12-48 hours, such as 12 hours or 24 hours.
[0046] In a third aspect, the present invention provides a use of the perfluoropolyether silane compound as described above as an anti-fingerprint oil, coating or surface treatment agent.
[0047] In a fourth aspect, the present invention provides a composite glass substrate, comprising a glass substrate and the perfluoropolyether silane compound as described above attached to the glass substrate.
[0048] In the present invention, the amount of the perfluoropolyether silane compound can be 24-36 g / m 2 , for example 30g / m 2 .
[0049] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0050] The reagents and raw materials used in the present invention are commercially available.
[0051] The positive and progressive effects of the present invention are:
[0052] (1) The core structure of the perfluoropolyether silane compound of the present invention is that the silane coupling agent is directly grafted onto the perfluoropolyether main chain through a chemical bond such as an amide bond, an ester bond or an imine bond, thereby improving its wear resistance on a glass substrate;
[0053] (2) The perfluoropolyether silane compound of the present invention has excellent hydrophobicity and oleophobicity;
[0054] (3) In the present invention, the preparation method of the perfluoropolyether silane compound is simple to operate and has a high product yield;
[0055] (4) The perfluoropolyether silane compound of the present invention has considerable application value in the field of anti-fingerprint oil, coating or surface treatment agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 To prepare the infrared spectrum of the perfluoropolyether alcohol in Example;
[0057] Figure 2 is the infrared spectrum of the perfluoropolyether silane compound in Example 1;
[0058] Figure 3 is the infrared spectrum of the perfluoropolyether silane compound in Example 2;
[0059] Figure 4 This is the infrared spectrum of the perfluoropolyether silane compound in Example 3. DETAILED DESCRIPTION
[0060] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0061] In the following examples and comparative examples, the specific details of the raw materials and equipment used are as follows:
[0062] K-type perfluoropolyether acyl fluoride: industrial grade, weight average molecular weight is about 3000g / mol, purchased from Suzhou Cangmu New Materials Co., Ltd., the structural formula is as follows:
[0063]
[0064] K-type perfluoropolyether methyl ester: industrial grade, weight average molecular weight is about 3000g / mol, purchased from Suzhou Cangmu New Materials Co., Ltd., the structural formula is as follows:
[0065]
[0066] 3-Aminopropyltrimethoxysilane: reagent grade, purchased from Shanghai Titan Technology Co., Ltd., with the following structural formula:
[0067]
[0068] 3-Chloropropyltrimethoxysilane: reagent grade, purchased from Shanghai Titan Technology Co., Ltd., with the following structural formula:
[0069]
[0070] 3-phenylaminopropyltrimethoxysilane: reagent grade, purchased from Shanghai Titan Technology Co., Ltd., with the following structural formula:
[0071]
[0072] 3-(Methacryloyloxy)propyltrimethoxysilane: reagent grade, purchased from Shanghai Titan Technology Co., Ltd., with the following structural formula:
[0073]
[0074] Tetrahydrofuran: reagent grade, purchased from Shanghai Titan Technology Co., Ltd.;
[0075] Thionyl chloride: reagent grade, purchased from Shanghai Titan Technology Co., Ltd.;
[0076] Lithium aluminum hydride: reagent grade, purchased from Shanghai Titan Technology Co., Ltd.;
[0077] Aluminum trichloride: reagent grade, purchased from Shanghai Titan Technology Co., Ltd.;
[0078] Sodium hydride: reagent grade, purchased from Shanghai Titan Technology Co., Ltd.;
[0079] Speier catalyst: reagent grade, purchased from Shanghai Titan Technology Co., Ltd.;
[0080] Fluorocarbon solvent DY30: purchased from Dongguan Dongyuan Optoelectronics Technology Co., Ltd.;
[0081] Automatic spraying machine: purchased from Dongguan Yingjie Intelligent Equipment Co., Ltd.;
[0082] Contact angle measuring instrument: purchased from Dongguan Kezhong Precision Instrument Co., Ltd.
[0083] Friction resistance tester: purchased from Dongguan Huaguo Precision Instrument Co., Ltd.
[0084] Preparation Example: Preparation of K-type perfluoropolyether alcohol
[0085] 228 mg of lithium aluminum hydride was added to 15 mL of tetrahydrofuran, and 226 mg of aluminum chloride was added in several times. After stirring for 10 minutes, 6.0 g of K-type perfluoropolyether methyl ester was added. After sufficient reaction, the mixture was repeatedly extracted and separated with a fluorocarbon solvent, and then the lower layer of liquid was taken and rotary evaporated to obtain K-type perfluoropolyether alcohol with a weight average molecular weight of about 2972 g / mol. The reaction process is as follows:
[0086]
[0087] See also Figure 1 In the infrared spectrum, the characteristic peak of the ester group of the raw material perfluoropolyether methyl ester disappeared, and the characteristic peak of the hydroxyl group was newly added in the product.
[0088] Example 1
[0089] 45.0 g (15.00 mmol) of type K perfluoropolyether acyl fluoride was added to 200 g of tetrahydrofuran, and then 3.8 g (14.88 mmol) of 3-phenylaminopropyltrimethoxysilane was added.
[0090] After reacting at 30°C for 24 hours, the mixture was repeatedly extracted and separated with a fluorocarbon solvent, and then the lower layer of liquid was taken and rotary evaporated to obtain a perfluoropolyether silane compound modified with 3-phenylaminopropyltrimethoxysilane, named anti-fingerprint oil 1, with a yield of 95%. The reaction process is as follows:
[0091]
[0092] See also Figure 2 In the infrared spectrum, the peak position of the carbonyl group in the product becomes smaller, indicating that the acyl fluoride has turned into an amide; the characteristic peak of the benzene ring also appears in the infrared of the product.
[0093] Example 2
[0094] 29.7 g (10.00 mmol) of the K-type perfluoropolyether alcohol prepared in the preparation example was added to 150 g of a fluorocarbon solvent, and then 5 mL of dichlorothionyl was added. After reacting at room temperature for 1 hour, the mixed solution was subjected to rotary evaporation. Then, 150 g of a fluorocarbon solvent was added to dissolve the product, and then 2.0 g (11.16 mmol) of 3-aminopropyltrimethoxysilane was added.
[0095] After reacting at 50°C for 12 hours, the mixture was repeatedly extracted and separated with a fluorocarbon solvent, and then the lower layer of liquid was taken and rotary evaporated to obtain a 3-aminopropyltrimethoxysilane-modified K-type perfluoropolyether anti-fingerprint oil, named anti-fingerprint oil 2, with a yield of 80%. The reaction process is as follows:
[0096]
[0097]
[0098] See also Figure 3 In the infrared spectrum, the characteristic peak of hydroxyl group of raw material K-type perfluoropolyether alcohol disappeared, and the characteristic peak of carbon-nitrogen single bond was newly added in the product.
[0099] Example 3
[0100] 30.0 g (10.00 mmol) of type K perfluoropolyether methyl ester was added to 150 g of tetrahydrofuran, and then 2.8 g (11.29 mmol) of 3-(methacryloyloxy)propyltrimethoxysilane was added.
[0101] After reacting at 30°C for 12 hours, the mixture was repeatedly extracted and separated with a fluorocarbon solvent, and then the lower layer of liquid was taken and rotary evaporated to obtain a perfluoropolyether silane compound modified with 3-(methacryloyloxy)propyltrimethoxysilane, named anti-fingerprint oil 3, with a yield of 91%. The reaction process is as follows:
[0102]
[0103] See also Figure 4 In the infrared spectrum, the characteristic peak of Si-OC is newly added to the product.
[0104] Comparative Example 1
[0105] 3.0 g of the K-type perfluoropolyether alcohol in the preparation example was added to 15 mL of tetrahydrofuran, and then 0.05 g of sodium hydride was added. After stirring at room temperature for 2 h, 0.14 g of allyl chloride was added. After sufficient reaction, Speier catalyst was added. 0.05 g of KH550 was added while stirring at a constant temperature of 60° C. After sufficient reaction, anti-fingerprint oil 4 was obtained. After sufficient reaction, fluorocarbon solvent was used for repeated extraction and separation, and then the lower layer of liquid was taken for rotary evaporation. The yield was 67%. The reaction process is as follows:
[0106]
[0107] Application Examples
[0108] The anti-fingerprint oils in Examples 1-3 and Comparative Example 1 were dissolved in fluorocarbon solvents at a ratio of 3‰, which is the ratio of the mass of the anti-fingerprint oil to the sum of the mass of the fluorocarbon solvent and the anti-fingerprint oil, to prepare surface treatment agents.
[0109] Use a sprayer to evenly spray the prepared surface treatment agent on the glass substrate with a spraying amount of 30g / m 2 , before spraying, the surface of the glass substrate needs to undergo conventional plasma treatment.
[0110] Then, the glass substrate sprayed with the surface treatment agent was placed in an oven at 165° C. for curing for 20 minutes, so that the surface treatment agent formed a paint film on the glass substrate.
[0111] Effect Example 1: Hydrophobic Performance Test
[0112] 1. Test object: the paint film made from the anti-fingerprint oil in Examples 1-3 and Comparative Example 1 in the application example.
[0113] 2. Test method: Use a contact angle meter to test the contact angle of water on the material surface, referring to the international test standard GB / T 24368-2009.
[0114] Effect Example 2: Oleophobic Performance Test
[0115] 1. Test object: the paint film made from the anti-fingerprint oil in Examples 1-3 and Comparative Example 1 in the application example.
[0116] 2. Test method: Use a contact angle meter to test the contact angle of n-hexadecane on the material surface, referring to the international test standard ASTM D5946-17.
[0117] Effect Example 3: Friction Resistance Test of Steel Wool
[0118] 1. Test object: the paint film made from the anti-fingerprint oil in Examples 1-3 and Comparative Example 1 in the application example.
[0119] 2. Test method: Use a friction tester to test the friction resistance of the paint film under the following conditions, and evaluate the water contact angle of the substrate surface after friction according to the test method of Example 1. The test is terminated when the number of frictions reaches 2500-3000 times. The parameters of the friction process are: Steel wool: Bonstar#0000 steel wool produced by Japan Steel Wool Co., Ltd. Load: 4kg / cm 2 . Friction stroke: 40mm. Friction speed: 40rpm.
[0120] The results of Effect Example 1 and Effect Example 3 are shown in Table 1.
[0121] Table 1 Hydrophobicity and wear resistance test results of anti-fingerprint oil
[0122]
[0123] The results of Effect Example 2 and Effect Example 3 are shown in Table 2.
[0124] Table 2 Oleophobic performance and wear resistance test results of anti-fingerprint oil
[0125]
[0126] In Examples 1-3, the silane coupling agent is directly connected to the K-type perfluoropolyether main chain through chemical bonds such as amide bonds, ester bonds or imine bonds, so that the anti-fingerprint oil has high wear resistance on the glass substrate and good adhesion. In Comparative Example 1, the silane coupling agent is connected to the K-type perfluoropolyether through a chain hydrocarbon group containing an ether bond. After 3000 frictions, the water contact angle of the surface of the material in Comparative Example 1 has a significant decline compared with that in Examples 1-3, and the contact angle of n-hexadecane has also declined.
Claims
1. A perfluoropolyether silane compound, characterized in that Its structural formula is as follows: Wherein, M' is methylene, M" is Alternatively, M' is carbonyl, M" is -O- or X', X" are each independently hydrogen, phenyl or the following groups: Y is a C1-C8 alkylene group, a C1-C8 heteroalkylene group, a C1-C8 alkylene group substituted with a substituent, or a C1-C8 heteroalkylene group substituted with a substituent; the heteroatom of the C1-C8 heteroalkylene group is O or N, and the number of heteroatoms is 1-2; the substituent is an epoxy group, a methacryloyloxy group, a phenyl group, an amino group or a halogen atom; Z" is a chemical bond, a phenylene group or an imino group; R', R", R'" are each independently a C1-C4 alkyl group; X' and X" are not hydrogen or phenyl at the same time; The average value of n is 6-100.
2. The perfluoropolyether silane compound according to claim 1, characterized in that It meets at least one of the following conditions ①-⑦: ①M' is a carbonyl group, M" is X" is a phenyl group; ②M' is methylene, M" is -NH-; ③M' is carbonyl, M" is -O-; ④Z" is a chemical bond, Y is a C1-C8 alkylene group, and the C1-C8 alkylene group is a C3 alkylene group, such as a C3 straight chain alkylene group; ⑤ The C1-C8 heteroalkylene group is ⑥ The epoxy group is an ethylene oxide or a propylene oxide; ⑦ R', R", and R'" are each independently a methyl group or an ethyl group.
3. The perfluoropolyether silane compound according to claim 1, characterized in that Its structural formula is one of the following ①-③: Among them, the average value of n is 16.1; Among them, the average value of n is 16.1; The average value of n is 16.
1.
4. The perfluoropolyether silane compound according to claim 1, characterized in that The average value of n is 10-20, for example, 16.1-18.0; and / or, Y is a C1-C8 alkylene group, such as a C3 alkylene group; And / or, the mass content of fluorine element in the perfluoropolyether silane compound is 50%-70%.
5. A method for preparing a perfluoropolyether silane compound as claimed in any one of claims 1 to 4, characterized in that: It includes the following steps: The K-type perfluoropolyether compound and the silane coupling agent are reacted in a first solvent.
6. The method for preparing a perfluoropolyether silane compound according to claim 5, characterized in that: The K-type perfluoropolyether compound is selected from one or more of K-type perfluoropolyether alcohol, K-type perfluoropolyether acyl chloride, K-type perfluoropolyether acyl fluoride and K-type perfluoropolyether methyl ester; and / or, the weight average molecular weight of the K-type perfluoropolyether compound is 1000-15000 g / mol, for example 2972 or 3000 g / mol; And / or, the silane coupling agent is selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, 3-phenylaminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane; And / or, the first solvent is tetrahydrofuran or a fluorocarbon solvent.
7. The method for preparing a perfluoropolyether silane compound according to claim 5, characterized in that: The molar ratio of the K-type perfluoropolyether compound to the silane coupling agent is 1:(0.9-1.2), for example, 15.00:14.88, 10.00:11.16 or 10.00:11.29; and / or, the dosage ratio of the K-type perfluoropolyether compound to the first solvent is 10.00 mmol:(150-200) g; and / or, the reaction temperature is 30-80°C, for example 30°C; And / or, the reaction time is 12-48 h, such as 12 h or 24 h.
8. Use of the perfluoropolyether silane compound as claimed in any one of claims 1 to 4 as an anti-fingerprint oil, coating or surface treatment agent.
9. A composite glass substrate, characterized in that: The invention comprises a glass substrate and the perfluoropolyether silane compound as claimed in any one of claims 1 to 4 attached to the glass substrate.
10. The composite glass substrate according to claim 9, characterized in that The amount of the perfluoropolyether silane compound is 24-36 g / m 2 , for example 30g / m 2 .
Citation Information
Cited By
Antibacterial type anti-fingerprint agent additive, preparation method and application thereof
CN122772012A