Preparation method and application of tackifying and shear strength improving agent
Through the reaction of catalyst and polymer with humic acid, a dendrimer modified humic acid viscosity enhancement and cutting agent was prepared, which solved the problem of lower viscosity of drilling fluid at high temperature and insufficient resistance to salt calcium at high temperatures, and achieved high temperatures Significant viscosity increase and improved suspension performance under conditions.
Patent Information
- Application Number
- CN202310664696.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
The existing drilling fluid desorption and dehydration of clay surface under high temperatures, resulting in a decrease in viscosity and shear force, and the temperature resistance of natural materials is insufficient. Synthetic polymer cutting agents are curled up in the brine. Loss of sticky ability.
The reaction of catalyst, polymer and humic acid is carried out to prepare a dendrimer-modified humic acid viscosity-enhancing and cutting agent, which has high branching and shear resistance, and can maintain viscosity under high temperature and salt calcium environment. and suspension performance.
It significantly improves the viscosity and shear force of the drilling fluid, improves rheology, and can maintain good rock carrying capacity under high temperature conditions. It is suitable for deep and low-rise oil and gas development.
Smart Images

Figure BDA0004284000620000031 
Figure BDA0004284000620000081 
Figure BDA0004284000620000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of drilling fluid, and in particular relates to a preparation method and application of a viscosity-enhancing and shear-enhancing agent. Background Art
[0002] Under high temperature conditions, the treatment agent produces desorption and dehydration on the clay surface, resulting in a weakened grid structure of the clay and the treatment agent, which reduces the viscosity and shear force of the drilling fluid and cannot meet the drilling requirements. The viscosity-enhancing and shear-enhancing agent can significantly increase the viscosity and shear force of the drilling fluid, improve the suspension capacity of the drilling fluid and improve the rheology of the drilling fluid. The currently used natural material modified products such as xanthan gum and modified cellulose are cheap and green, but have insufficient temperature resistance (<140°C); the molecular chains of linear synthetic polymer viscosity-enhancing and shear-enhancing agents are easily affected by cations in saturated brine and composite brine drilling fluids, resulting in molecular chain curling, thereby losing the viscosity-enhancing and shear-enhancing ability. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide a preparation method and application of a viscosity-enhancing and shear-enhancing agent. The viscosity-enhancing and shear-enhancing agent prepared by the present invention has good temperature resistance, salt and calcium resistance, and shear resistance.
[0004] The present invention provides a method for preparing a viscosity-increasing and shear-improving agent, comprising:
[0005] mixing the catalyst, the polymer and the humic acid to obtain a mixed solution;
[0006] The mixed liquid is reacted to obtain a dendrimer-modified humic acid viscosity-enhancing and shear-enhancing agent for water-based drilling fluid.
[0007] In an embodiment of the present invention, the catalyst may be selected from one or more of trifluoroacetic acid, sulfuric acid, and p-toluenesulfonic acid.
[0008] In an embodiment of the present invention, the polymer can be selected from a dendrimer, and the active groups at the polymer end groups can be selected from primary amine groups and / or secondary amine groups; the number of active groups at the end groups can be selected from 4 to 32, such as 5, 10, 15, 20, 25, 30.
[0009] In an embodiment of the present invention, the method for preparing a polymer may include:
[0010] The polyamine solution and the acrylate are subjected to a first reaction to obtain a reaction product;
[0011] The solution of the reaction product is subjected to a second reaction with a polyamine to obtain a polymer.
[0012] In an embodiment of the present invention, the first reaction may be performed under the condition of a protective gas, and the protective gas may be selected from nitrogen.
[0013] In an embodiment of the present invention, the polyamine in the polyamine solution may be selected from one of ethylenediamine, diethanolamine, diethylenetriamine and triethylenetetramine.
[0014] In an embodiment of the present invention, the solvent in the polyamine solution can be selected from methanol; the mass concentration of the polyamine solution can be selected from 5 to 50%, such as 10%, 20%, 30%, and 40%.
[0015] In the embodiment of the present invention, the acrylate may be selected from one or more of methyl acrylate, methyl methacrylate, and ethyl acrylate.
[0016] In an embodiment of the present invention, the molar ratio of polyamine to acrylate in the polyamine solution can be selected from (4-6): (16-32), such as (4.5-5.5): (20-30), 5:25.
[0017] In an embodiment of the present invention, the temperature of the first reaction may be no higher than 25°C, and may be selected from 20 to 25°C, such as 22°C, 23°C; the time of the first reaction may be selected from 24 to 48h, such as 36h.
[0018] In an embodiment of the present invention, after the first reaction is completed, the following steps are further included:
[0019] The obtained reaction product is distilled under reduced pressure to obtain a half-generation dendritic polymer.
[0020] In an embodiment of the present invention, the second reaction may be performed under the condition of a protective gas, and the protective gas may be selected from nitrogen.
[0021] In an embodiment of the present invention, the solvent in the solution of the reaction product can be selected from methanol, and the mass concentration of the solution of the reaction product can be selected from 5 to 55%, such as 10%, 20%, 30%, 40%, 50%.
[0022] In an embodiment of the present invention, the polyamine may be selected from one of ethylenediamine, diethanolamine, diethylenetriamine and triethylenetetramine.
[0023] In an embodiment of the present invention, the polyamine in the first reaction and the polyamine in the second reaction may be the same or different.
[0024] In an embodiment of the present invention, the molar ratio of the reaction product to the polyamine can be selected from (8-12): (16-24), such as (9-11): (18-22), 10:20.
[0025] In an embodiment of the present invention, the temperature of the second reaction may be no higher than 25°C, and may be selected from 20 to 25°C, such as 22°C, 23°C; the time of the second reaction may be selected from 24 to 60h, such as 36h, 48h.
[0026] In an embodiment of the present invention, after the second reaction is completed, the following steps are further included:
[0027] The obtained reaction product was distilled under reduced pressure to obtain an oily dendrimer.
[0028] In an embodiment of the present invention, the method for preparing a polymer may include:
[0029] Under nitrogen protection, polyamine is dissolved in methanol, acrylate is slowly added, the temperature is controlled not higher than 25°C, the reaction is carried out for 24 to 48 hours, and after the reaction is completed, the half-generation dendritic polymer is obtained by vacuum distillation;
[0030] Under nitrogen protection, the half-generation dendrimer is dissolved in methanol, polyamine is slowly added, the temperature is controlled not higher than 25°C, the reaction is carried out for 24 to 60 hours, and after the reaction is completed, the oily dendrimer is obtained by vacuum distillation.
[0031] In the embodiment of the present invention, the humic acid may be industrial humic acid.
[0032] In an embodiment of the present invention, the mass of the catalyst can be 0.1-5% of the total mass of the polymer and humic acid, such as 0.5%, 1%, 2%, 3%, 4%; the mass ratio of the polymer and humic acid can be selected from (1-4): (5-1), such as (2-3): (4-2), 2.5:3.
[0033] In an embodiment of the present invention, the mixed solution can be reacted under closed conditions, and the reaction temperature can be selected from 100 to 150°C, such as 110°C, 120°C, 130°C, and 140°C; the reaction time can be selected from 0.5 to 8h, such as 1h, 2h, 3h, 4h, 5h, 6h, and 7h.
[0034] In an embodiment of the present invention, the mixed liquid may further include: a solvent; the solvent may be selected from water, such as deionized water, distilled water, and tap water.
[0035] In an embodiment of the present invention, after the mixed solution is reacted, the following steps may further be included:
[0036] The obtained reaction product is discharged, cooled, dried and crushed to obtain a black powder product.
[0037] In an embodiment of the present invention, the preparation method of the (tree polymer modified humic acid for water-based drilling fluid) viscosity increasing and shearing improving agent may include:
[0038] Add an appropriate amount of solvent to a reaction kettle equipped with a stirrer, a gas protection device and a temperature controller, add the required weight of polymer under stirring until it is completely dissolved, continue to add 0.25 to 2 parts of humic acid, and finally add 0.1 to 5% of a catalyst to react; control the reaction temperature to 100 to 150° C. and the reaction time to 0.5 to 8.0 hours; after the reaction is completed, discharge the material, cool, dry, and crush to obtain a black powder product.
[0039] In an embodiment of the present invention, the schematic diagram of the structure of the salt-calcium-resistant and high-temperature-resistant dendrimer-modified humic acid shearing agent (dendrimer-modified humic acid thickening and shearing agent for water-based drilling fluid) is as follows:
[0040]
[0041] Among them, Hm represents humic acid molecule and PAMAM represents dendrimer.
[0042] In the embodiments of the present invention, the dendrimer has the characteristics of high branching degree, strong shear resistance and a large number of terminal active groups; humic acid has the characteristics of many rigid structures, many active reaction groups and strong temperature resistance; humic acid and a dendrimer with an amino terminal group are reacted to obtain a product that has both the strong temperature resistance of humic acid and the high branching degree of the dendrimer, and has good high-temperature shear ability, which significantly improves the rock-carrying capacity of freshwater drilling fluid, saturated brine drilling fluid, composite brine drilling fluid and polymer drilling fluid under high temperature conditions, and is of great significance to the development of deep low-layer oil and gas.
[0043] The present invention provides a drilling fluid, comprising: a viscosity-enhancing and shear-enhancing agent prepared by the method described in the above technical solution.
[0044] In an embodiment of the present invention, the mass content of the viscosity increasing and shear enhancing agent in the drilling fluid can be selected from 0.1-1%, such as 0.2%, 0.5%, 0.8%.
[0045] In an embodiment of the present invention, the drilling fluid can be selected from a polymer freshwater-based slurry, a freshwater-based slurry, a saturated saltwater-based slurry, and a composite saltwater-based slurry. In an embodiment of the present invention, the polymer freshwater-based slurry may include: bentonite, sodium carbonate, water, and a polymer fluid loss reducer; bentonite, sodium carbonate; the amount ratio of water and polymer fluid loss reducer may be selected from (15-25) g: (0.5-0.9) g: (350-450) mL: (2-6) g, such as (18-22) g: (0.6-0.8) g: (380-420) mL: (3-5) g, 20 g: 0.7 g: 400 mL: 4 g; the preparation method may include: adding bentonite and sodium carbonate to water, stirring, standing, adding a polymer fluid loss reducer under stirring, stirring and standing to obtain a polymer freshwater-based slurry; the stirring speed may be selected from 6000-10000 r / min, such as 8000 r / min; the stirring time can be selected from 15 to 25 minutes, such as 20 minutes; the standing time can be selected from 20 to 30 hours, such as 24 hours; the rotation speed in the stirring state can be selected from 6000 to 10000 r / min, such as 8000 r / min; the stirring time can be selected from 15 to 25 minutes, such as 20 minutes; the standing time can be selected from 20 to 30 hours, such as 24 hours; the preparation method of the drilling fluid may include: adding the (water-based drilling fluid tree polymer modified humic acid) viscosity increasing and shearing agent to the polymer fresh water base slurry and stirring to obtain the drilling fluid; the stirring speed can be selected from 6000 to 10000 r / min, such as 8000 r / min; the stirring time can be selected from 15 to 25 minutes, such as 20 minutes.
[0046] In an embodiment of the present invention, the fresh water-based slurry may include: bentonite, sodium carbonate and water; the usage ratio of bentonite, sodium carbonate and water may be selected from (14-20) g: (0.5-0.6) g: (350-450) mL, such as (15-17) g: (0.52-0.58) g: (380-420) mL, 16 g: 0.56 g: 400 mL; the preparation method of the fresh water-based slurry may include: stirring bentonite, sodium carbonate and water, and standing to obtain the fresh water-based slurry; The stirring speed can be selected from 6000 to 10000 r / min, such as 8000 r / min; the standing time can be selected from 20 to 30 hours, such as 24 hours; the preparation method of the drilling fluid comprises: adding the water-based drilling fluid tree polymer modified humic acid viscosity enhancing and shearing agent to the fresh water-based slurry and stirring to obtain the drilling fluid; the stirring speed can be selected from 6000 to 10000 r / min, such as 8000 r / min; the stirring time can be selected from 15 to 25 minutes, such as 20 minutes.
[0047] In an embodiment of the present invention, the saturated salt water base slurry may include: water, sodium carbonate, bentonite and sodium chloride; the water may be selected from distilled water; the sodium carbonate may be selected from anhydrous sodium carbonate; the bentonite may be selected from bentonite for drilling fluid test slurry; the usage ratio of water, sodium carbonate, bentonite and sodium chloride may be selected from (300-400) mL: (0.45-0.55) g: (10-20) g: (110-140) g, such as (330-370) mL: (0.48-0.52) g: (12-18) g: (120-130) g, 350 mL: 0.49 g: 14 g: 126 g; the preparation method of the saturated salt water base slurry may include: stirring water, sodium carbonate and bentonite and then performing a first curing, adding sodium chloride, performing high-speed stirring and then performing a second curing to obtain the saturated salt water base slurry; the stirring may be performed in a high-speed mixer, The stirring speed can be selected from 10000~12000r / min, such as 11000r / min; the stirring time can be selected from 15~25min, such as 20min; stop at least twice during the stirring process to scrape off the clay adhering to the container wall; the first curing can be selected from closed curing, the temperature of the first curing can be selected from room temperature, and the time of the first curing can be selected from 20~30h, such as 24h; the time of high-speed stirring can be selected from 15~25min, such as 20min; stop at least twice during the high-speed stirring to scrape off the clay adhering to the container wall; the second curing can be selected from closed curing; the temperature of the second curing can be selected from room temperature; the time of the second curing can be selected from 20~30h; the API filtration loss of the saturated salt water slurry after rolling at 200℃ for 16h needs to be within the range of 200~250mL, otherwise the amount of bentonite added needs to be adjusted.
[0048] In an embodiment of the present invention, the composite salt water-based slurry may include: water, sodium chloride, calcium chloride, magnesium chloride, bentonite, and sodium carbonate; water may be selected from distilled water; calcium chloride may be selected from anhydrous calcium chloride; bentonite may be selected from bentonite for drilling fluid test slurry; sodium carbonate may be selected from anhydrous sodium carbonate; the usage ratio of water, sodium chloride, calcium chloride, magnesium chloride, bentonite and sodium carbonate may be selected from (300-400) mL: (10-20) g: (1.5-2) g: (3-8) g: (45-55) g: (2-4) g, such as (330-370) mL: (14-18) g: (1.7-1.8) g: (4-5) g: (48-53) g: (2.5-3.5) g. 0mL: 16g: 17.5g: 4.6g: 52.5g: 3.15g; The preparation method of the composite salt water-based slurry may include: stirring water, sodium chloride, calcium chloride, magnesium chloride, bentonite, and sodium carbonate at high speed and then curing; The speed of high-speed stirring is selected from 10000-12000r / min, such as 11000r / min; The time of high-speed stirring is selected from 15-25min, such as 20min; Stop at least twice during high-speed stirring to scrape off the clay adhering to the container wall; The curing temperature can be selected from 22-28℃, such as 25℃; The curing time can be selected from 20-30h, such as 24h; Curing can be selected from closed curing; The composite salt water-based slurry is stirred at high speed for 5min, and its filtration loss (GB / T 16783.1 standard test) needs to be 80-100mL. Otherwise, the amount of bentonite added needs to be adjusted.
[0049] In order to solve the problem that natural product shearing agents have insufficient temperature resistance and synthetic polymer shearing agents have insufficient salt, calcium and shear resistance, the present invention provides a temperature-resistant, salt-calcium-resistant and shear-resistant water-based drilling fluid viscosity-enhancing and shearing agent, specifically a tree polymer modified humic acid viscosity-enhancing and shearing agent for water-based drilling fluid, and a preparation method and application thereof.
[0050] The salt-calcium-resistant and high-temperature-resistant dendrimer modified humic acid shearing agent provided by the present invention is formed by the grafting reaction of a dendrimer and humic acid, has simple conditions, is easy to operate, and has high reaction efficiency. The product shows a significant shearing effect in different types of drilling fluids, and can solve the problems of decreased viscosity and poor suspension of freshwater drilling fluid, saturated brine drilling fluid, composite brine drilling fluid and polymer drilling fluid under high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is the infrared spectrum of the product prepared in Example 1 of the present invention;
[0052] Figure 2 is the infrared spectrum of humic acid in Example 2 of the present invention;
[0053] Figure 3This is the infrared spectrum of the product prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The humic acid used in the following examples of the present invention is a humic acid ore product provided by Huolinguole Wolong Biotechnology Co., Ltd.
[0056] Example 1
[0057] Under nitrogen protection and stirring, 60.10 kg of ethylenediamine was dissolved in 1200 kg of methanol, the solution temperature was controlled at 20-25°C, and then 344.36 kg of methyl acrylate was slowly added, the temperature was controlled at 20-25°C, and the reaction was carried out for 24 hours; after the reaction was completed, the half-generation dendritic polymer was obtained by vacuum distillation, and methanol was recovered;
[0058] Under nitrogen protection and stirring conditions, 404 kg of the half-generation dendrimer prepared above was dissolved in 2000 kg of methanol, 240.4 kg of ethylenediamine was slowly added, the solution temperature was controlled at 20-25° C., and the reaction was carried out for 48 hours; after the reaction was completed, vacuum distillation was performed to obtain a dendrimer raw material.
[0059] The product prepared in Example 1 was subjected to infrared spectroscopy detection. Figure 1 As shown, it can be seen that it has functional groups such as amide group and amino group.
[0060] Example 2
[0061] In parts by weight, 200 parts of deionized water were added to a reactor equipped with a stirrer, a temperature controller and an air duct, and 200 parts of the dendrimer prepared in Example 1 were added under stirring. After stirring until the dendrimer was completely dissolved, 60 parts of humic acid and 1.25 parts of p-toluenesulfonic acid were added. The reaction temperature was controlled to be 140° C. and the reaction was carried out for 2.0 hours. After the reaction was completed, the material was discharged, cooled, dried and crushed to obtain a black powder product.
[0062] Compare the infrared spectrum of humic acid and the infrared spectrum of the product prepared in Example 2 ( Figure 2 and Figure 3 ), it can be seen that the carboxyl signal in humic acid is reduced and the amide signal is enhanced, proving that the dendrimer and humic acid react in Example 2 to obtain a viscosity-enhancing and shear-enhancing agent.
[0063] Example 3
[0064] In parts by weight, 200 parts of deionized water were added to a reactor equipped with a stirrer, a temperature controller and an air duct, and 200 parts of the dendritic polymer prepared in Example 1 were added under stirring. After stirring until the dendritic polymer was completely dissolved, 120 parts of humic acid and 1.25 parts of sulfuric acid were added. The reaction temperature was controlled to be 140° C. and the reaction was carried out for 3.0 hours. After the reaction was completed, the material was discharged, cooled, dried and crushed to obtain a black powder product.
[0065] Example 4
[0066] In parts by weight, 200 parts of deionized water were added to a reactor equipped with a stirrer, a temperature controller and an air duct, and 200 parts of the dendrimer prepared in Example 1 were added under stirring. After stirring until the dendrimer was completely dissolved, 200 parts of humic acid and 1.25 parts of p-toluenesulfonic acid were added. The reaction temperature was controlled to be 150° C. and the reaction was carried out for 3.0 hours. After the reaction was completed, the material was discharged, cooled, dried and crushed to obtain a black powder product.
[0067] Example 5
[0068] In parts by weight, 200 parts of deionized water were added to a reaction kettle equipped with a stirrer, a temperature controller and an air duct, and 200 parts of the dendrimer prepared in Example 1 were added under stirring. After stirring until the dendrimer was completely dissolved, 300 parts of humic acid and 2.5 parts of p-toluenesulfonic acid trifluoroacetic acid were added. The reaction temperature was controlled to be 150° C. and the reaction was carried out for 5.0 hours. After the reaction was completed, the material was discharged, cooled, dried and crushed to obtain a black powder product.
[0069] Performance Testing
[0070] The performance of the salt-calcium-resistant and high-temperature-resistant dendrimer-modified humic acid shearing agent (black powder product) prepared in the example was evaluated in a polymer freshwater-based slurry. The preparation method of the polymer freshwater-based slurry is as follows: 20g of bentonite (Bohai drilling soil) and 0.7g of sodium carbonate (provided by Tianjin Komeo) were added to 400mL of water, stirred at 8000r / min for 20min, and allowed to stand for 24h. Then, 4.0g of EHBPS-H (polymer viscosity-enhancing and filtration-reducing agent, provided by Zhongyuan Drilling Institute) was added under stirring at 8000r / min, stirred for 20min, and allowed to stand for 24h to obtain a polymer freshwater-based slurry as a blank control.
[0071] The salt-calcium-resistant and high-temperature-resistant dendritic polymer modified humic acid shearing agent (black powder product) prepared in Examples 2 to 5 was added to the above-mentioned polymer freshwater slurry in an amount of 0.5% of the mass of the polymer drilling fluid base slurry. The mixture was stirred at a speed of 8000 r / min for 20 min to obtain a polymer freshwater slurry to be evaluated containing 0.5% of the shearing agent.
[0072] The performance parameters such as apparent viscosity AV, plastic viscosity PV, dynamic shear force YP and dynamic plastic ratio J of the blank control slurry and the polymer slurry containing the shearing agent after hot rolling aging at room temperature and 150℃ for 16h were measured and calculated. The changes in parameters such as the viscosity of the shearing agent solution before and after aging were compared. The change range of these parameters was used as an indicator to evaluate the heat resistance of the shearing agent. The test results are as follows:
[0073]
[0074] It can be seen that the viscosity increasing and shearing enhancing agent has a significant viscosity increasing and shearing enhancing effect on the polymer drilling fluid. After high-temperature aging at 150°C, compared with the blank control, the apparent viscosity and dynamic shear force of Examples 2 to 5 are significantly improved, which can well meet the suspension requirements of the drilling fluid.
[0075] The performance of the salt-calcium-resistant and high-temperature-resistant dendrimer-modified humic acid shearing agent (black powder product) prepared in the example was evaluated in 4% fresh water-based slurry. The preparation method of 4% fresh water-based slurry is as follows: 16g of bentonite (Bohai drilling soil) and 0.56g of sodium carbonate (provided by Tianjin Komio) were added to 400mL of water, stirred at 8000r / min for 20min, and after standing for 24h, 4% fresh water-based slurry was obtained as a blank control.
[0076] The salt-calcium-resistant and high-temperature-resistant dendrimer modified humic acid shearing agent (black powder product) prepared in Example 4 was added to the above-mentioned 4% fresh water base slurry in an amount of 0.5% of the mass of the 4% fresh water base slurry. The mixture was stirred at a speed of 8000 r / min for 20 minutes to obtain the fresh water base slurry to be evaluated containing 0.5% of the shearing agent.
[0077] The performance parameters such as apparent viscosity AV, plastic viscosity PV, dynamic shear force YP and dynamic plastic ratio J of the blank control slurry and the fresh water slurry containing 4% shearing agent after hot rolling aging at room temperature and 180℃ for 16h were measured and calculated. The changes in the viscosity of the shearing agent solution before and after aging were compared. The change range of these parameters was used as an indicator to evaluate the heat resistance of the shearing agent. The test results are as follows:
[0078]
[0079] It can be seen that the viscosity increasing and shearing enhancing agent has a significant viscosity increasing and shearing enhancing effect on the 4% fresh water base slurry. After high temperature aging at 180°C, compared with the blank control, the apparent viscosity of Example 4 is significantly improved, which can well meet the suspension requirements of the drilling fluid.
[0080] The performance of the salt-calcium-resistant and high-temperature-resistant dendrimer-modified humic acid shearing agent (black powder product) prepared in the embodiment was evaluated in a saturated salt water base slurry. The preparation method of the saturated salt water base slurry is as follows: in a high stirring cup filled with 350 mL of distilled water, 0.49 g of anhydrous sodium carbonate and 14.0 g of bentonite for drilling fluid test slurry were added, and stirred at a speed of 11,000 r / min for 20 min with a high-speed stirrer, and stopped at least twice during the stirring to scrape off the clay adhering to the container wall. After sealed curing at room temperature for 24 h, 126 g of NaCl was added, and stirred at high speed for 20 min, and stopped at least twice during the stirring to scrape off the clay adhering to the container wall. The saturated salt water base slurry was used as the API filtration loss of the base slurry after rolling at 200° C. for 16 h should be within the range of 200 mL to 250 mL, otherwise the amount of bentonite for drilling fluid test slurry should be adjusted.
[0081] The salt-calcium-resistant and high-temperature-resistant dendritic polymer modified humic acid shearing agent (black powder product) prepared in Example 4 was added to the above-mentioned saturated brine base slurry in an amount of 0.5% of the mass of the saturated brine base slurry. The mixture was stirred at a speed of 8000 r / min for 20 minutes to obtain the saturated brine base slurry to be evaluated containing 0.5% of the shearing agent.
[0082] The performance parameters such as apparent viscosity AV, plastic viscosity PV, dynamic shear force YP and dynamic plastic ratio J of the blank control saturated brine slurry and the saturated brine slurry containing the shearing agent were measured and calculated after hot rolling aging at room temperature and 180℃ for 16h. The changes in parameters such as the viscosity of the shearing agent solution before and after aging were compared. The change range of these parameters was used as an indicator to evaluate the heat resistance of the shearing agent. The test results are as follows:
[0083]
[0084] It can be seen that the viscosity increasing and shearing enhancing agent has a significant viscosity increasing and shearing enhancing effect on the saturated salt water base slurry. After high temperature aging at 180°C, the apparent viscosity of Example 4 is significantly improved compared with the blank control.
[0085] The salt-calcium-resistant and high-temperature-resistant dendrimer-modified humic acid shearing agent (black powder product) prepared in Example 4 was added to the composite salt water base slurry. The preparation method of the composite salt water base slurry was as follows: 350 mL of distilled water was measured and placed in a high-stirring cup, 16.0 g of sodium chloride, 1.75 g of anhydrous calcium chloride, and 4.6 g of magnesium chloride were added, and after all of them were dissolved, 52.5 g of bentonite for drilling fluid test slurry and 3.15 g of anhydrous sodium carbonate were added, and the mixture was stirred at a speed of 11,000 r / min for 20 min with a high-speed stirrer, and the mixture was stopped at least twice to scrape off the clay adhering to the container wall, and the mixture was sealed and cured at (25±3)°C for 24 h as the composite salt water base slurry. The base slurry was stirred at high speed for 5 min, and the mixture was stirred according to GB / T 16783.1 stipulates that the API filtration loss should be measured and controlled within 80mL~100mL, otherwise the amount of bentonite added for drilling fluid test slurry should be adjusted; the added amount is 0.5% of the mass of the composite brine base slurry, and stirred at a speed of 8000r / min for 20min to obtain the composite brine base slurry to be evaluated containing 0.5% of the shear enhancement agent.
[0086] The performance parameters such as apparent viscosity AV, plastic viscosity PV, dynamic shear force YP and dynamic plastic ratio J of the blank control composite brine-based slurry and the composite brine-based slurry containing the shearing agent after hot rolling aging at room temperature and 180°C for 16 hours were measured and calculated. The changes in parameters such as the viscosity of the shearing agent solution before and after aging were compared. The changes in these parameters were used as indicators for evaluating the heat resistance of the shearing agent. The test results are as follows:
[0087]
[0088] It can be seen that the viscosity increasing and shearing enhancing agent has a significant viscosity increasing and shearing enhancing effect on the composite salt water-based slurry. After high-temperature aging at 180°C, the apparent viscosity of Example 4 is significantly improved compared with the blank control.
[0089] The salt-calcium-resistant and high-temperature-resistant dendrimer modified humic acid shearing agent provided by the present invention is formed by the grafting reaction of a dendrimer and humic acid, has simple conditions, is easy to operate, and has high reaction efficiency. The product shows a significant shearing effect in different types of drilling fluids, and can solve the problems of decreased viscosity and poor suspension of freshwater drilling fluid, saturated brine drilling fluid, composite brine drilling fluid and polymer drilling fluid under high temperature conditions.
[0090] Although the present invention has been described and illustrated with reference to specific embodiments of the present invention, these descriptions and illustrations do not limit the present invention. It will be clearly understood by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention as defined by the appended claims, so that specific circumstances, materials, material compositions, materials, methods or processes are suitable for the goals, spirit and scope of the present application. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to specific operations performed in a specific order, it should be understood that these operations may be combined, subdivided or reordered to form equivalent methods without departing from the teachings of the present invention. Therefore, unless specifically indicated herein, the order and grouping of operations are not limitations of the present application.
Claims
1. A method for preparing a viscosity-increasing and shear-enhancing agent, comprising: mixing the catalyst, the polymer and the humic acid to obtain a mixed solution; The mixed solution is reacted to obtain a viscosity-enhancing and shear-enhancing agent.
2. The preparation method according to claim 1, characterized in that: The catalyst is selected from one or more of trifluoroacetic acid, sulfuric acid and p-toluenesulfonic acid.
3. The preparation method according to claim 1, characterized in that: The preparation method of the polymer comprises: The polyamine solution and the acrylate are subjected to a first reaction to obtain a reaction product; The solution of the reaction product is subjected to a second reaction with polyamine to obtain a polymer.
4. The preparation method according to claim 3, characterized in that: The polyamine solution is selected from a methanol solution of polyamine; and the mass concentration of the polyamine solution is selected from 5 to 50%.
5. The preparation method according to claim 3, characterized in that: The polyamine in the polyamine solution is selected from one of ethylenediamine, diethanolamine, diethylenetriamine and triethylenetetramine; The polyamine is selected from one of ethylenediamine, diethanolamine, diethylenetriamine and triethylenetetramine.
6. The preparation method according to claim 3, characterized in that: The acrylic acid ester is selected from one or more of methyl acrylate, ethyl acrylate and methyl methacrylate.
7. The preparation method according to claim 3, characterized in that: The solvent in the solution of the reaction product is selected from methanol; The mass concentration of the solution of the reaction product is selected from 5 to 55%.
8. The preparation method according to claim 1, characterized in that: The mass of the catalyst is 0.1-5% of the total mass of the polymer and humic acid; The mass ratio of the polymer to humic acid is selected from (1-4): (5-1).
9. The preparation method according to claim 1, characterized in that: The reaction temperature is selected from 100 to 150° C.; the reaction time is selected from 0.5 to 8 hours.
10. A drilling fluid comprising: The viscosity-enhancing and shear-enhancing agent prepared by the method according to claim 1.