Preparation method of eggshell calcium-based organic iron optical screen salt absorption and pollution reduction composite material

By pretreating urea and organic acid on the eggshell, combined with iron salt and fumaric citric acid, an eggshell calcium-based organic iron light shielding salt absorption and pollution reduction composite material was prepared, which solved the insufficient binding degree of straw material activity center Problem, it realizes the degradation of highly efficient adsorbed salt ions and organic pollutants, and provides an inexpensive environmental restoration material.

CN119081138APending Publication Date: 2024-12-06SHIHEZI UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411182781.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The active center of the existing straw/MIL-88A composite material is not bound to the straw fibers, resulting in diffusion and loss of the active center, low loading rate, affecting the stability and long-term effectiveness of the material.

Method used

The eggshell is pretreated with a mixed solution of urea and organic acid to increase its porosity and load capacity, and the iron salt composite solution is added, and hydrogen bond protection formed by ultrasonic mixing and urea is prepared by combining fumaric acid and citric acid. Eggshell calcium-based organic iron light shielding salt absorption and pollution reduction composite material.

Benefits of technology

Under non-light conditions, the material can efficiently adsorb salt ions and degrade organic pollutants, improve the stability and long-term effectiveness of the composite material, and provide an inexpensive environmental restoration material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081138A_ABST
    Figure CN119081138A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of environmental pollution control, and discloses a preparation method of an eggshell calcium-based organic iron optical screen salt absorption and pollution reduction composite material. The method comprises the following steps: pretreating eggshells by using a mixed solution of urea and organic acid, adding a ferric salt composite solution in a certain proportion, carrying out ultrasonic mixing, and reacting at a certain temperature to prepare the eggshell calcium-based organic iron photosensitization salt-absorbing pollution-reducing composite material. Meanwhile, organic pollutants can be efficiently degraded under dark reaction, and the material is a cheap environment function repairing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental pollution control and relates to a method for preparing an eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material. Background Art

[0002] Eggshells contain about 85% CaCO3 and about 15% protein, as well as trace elements such as zinc, copper, manganese, iron and selenium. Eggshells themselves have a microporous structure, and their own structure is stable, with little pollution to the environment, and can be used as an excellent adsorption material. For example, eggshells can be synthesized into hydrotalcite eggshell composites with magnetic functions by a one-step foaming method. This material can adsorb small molecules of carbon sources in waste sludge and alleviate the risk of eutrophication of sewage. The eggshells are pretreated with organic acids such as acetic acid and citric acid, and Al2O3 in different proportions is doped by the sol-gel combustion synthesis method to prepare energy storage materials with recyclable adsorption. Therefore, eggshells, as a natural high-calcium substance, can be modified to prepare various composite materials with adsorption capacity.

[0003] In recent years, more and more organic ligands and inorganic metal ions can form metal organic framework materials through self-assembly. This material has the characteristics of ultra-large specific surface area, open pore channels and easy post-modification. Patent CN200480004726.7 discloses an iron organic compound, its application and its preparation method, by adding sodium hydroxide to ferric chloride, then adding citric acid, heating reaction, and preparing ferric citrate solution. Patent CN202110655106.5 discloses the preparation of a straw / MIL-88A composite material and the application of activated sodium persulfate to degrade pesticides in soil. An organic metal framework material with catalytic function is synthesized using fumaric acid and ferric chloride hexahydrate, and a straw / MIL-88A composite material is prepared by adding straw powder to the reaction phase. The material can activate persulfate to degrade pesticide pollutants at room temperature, but the active center of the material is not sufficiently bound to the straw fiber, and it is easy to diffuse and lose the active center of the organic metal framework. This is mainly because the surface structure of the straw material itself is dense, the proportion of active functional groups is small, the binding force with the active center is weak, and the loading rate is low. Therefore, how to break the dense structure of the straw, increase the active components on the surface of the straw, and improve the loading rate and binding degree of the organic metal framework material is the key to increasing the stability and long-term effectiveness of the composite material.

[0004] Based on the above analysis, the present invention will use a mixed solution of urea and organic acid to pretreat the eggshell to improve the porosity and loading capacity of the eggshell, and then add a certain proportion of an iron salt composite solution to increase the binding degree of iron ions and eggshell calcium through the hydrogen bond protection formed by urea. After ultrasonic mixing, a composite organic acid ligand is added to react under certain temperature conditions to prepare an eggshell calcium-based organic iron light-shielding salt-absorbing and pollution-reducing composite material. The composite material can adsorb salt ions under non-light conditions and effectively degrade organic pollutants, and can be used as a cheap environmental remediation material. Summary of the invention

[0005] The present invention uses discarded eggshells to establish a method for preparing an eggshell calcium-based organic iron light-shielding salt absorption and pollution reduction composite material. The eggshell is pretreated with a mixed solution of urea and an organic acid, a certain proportion of an iron salt composite solution is added, and after ultrasonic mixing, the mixture is reacted at a certain temperature to prepare an eggshell calcium-based organic iron light-shielding salt absorption and pollution reduction composite material. The composite material can shield the adsorption capacity of the composite material under natural light, and can efficiently degrade organic pollutants under dark reaction, and is a cheap environmental functional repair material.

[0006] The technical solution of the present invention:

[0007] A method for preparing an eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material, the steps are as follows:

[0008] The dried eggshells are crushed to 40-100 meshes, and a mixed solution of urea, oxalic acid and prohexadione is added, wherein the mass ratio of the eggshell to the mixed solution is controlled to be 1:(10-20), and ultrasonic treatment is performed for 3-5 minutes, and the mixture is reacted at 50-60° C. for 2-5 hours to obtain an eggshell calcium-based nitrogen-containing complex having a porous structure; iron pyrophosphate of 1-5% of the mass of the eggshell is added to the eggshell calcium-based nitrogen-containing complex, and the mixture is ultrasonically treated for 3-5 minutes, and the mixture is cultured on a constant temperature oscillator at 40-50° C. and 180 r / min for 3-4 hours to allow the iron ions to fully react with the eggshell calcium. The nitrogen-containing complex is bonded by urea amino hydrogen bonds; then, fumaric acid and citric acid are added into a mixed solid in a ratio of 1%-10% and 1%-5% by weight of the eggshell, respectively, and ultrasonic treatment is performed for 3-5 minutes, the ultrasonic temperature is room temperature, the frequency is 20kHz, and the reaction is performed at 80-120°C for 3-8 hours. After standing and cooling to room temperature, the solid-liquid separation is performed, and the solid is washed three times in sequence with anhydrous ethanol and ultrapure water respectively. After the obtained solid is dried in a blast drying oven at 60°C for 8-10 hours, it is ground into powder to obtain the eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material.

[0009] The masses of the urea, oxalic acid and prohexadione are 1-2%, 0.1-1% and 2%-5% of the mass of the mixed aqueous solution respectively.

[0010] The above-obtained eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material is applied, and the composite material is fully mixed with wastewater containing salt or organic pollutants at a mass ratio of 1: (50-200). For wastewater containing organic pollutants, sodium persulfate needs to be additionally added at a ratio of 0.1%-0.5% of the wastewater mass. The reaction is carried out under non-light conditions for 5-10 hours, and the salt content or the amount of organic pollutants in the water body is regularly measured.

[0011] The saline wastewater includes Na + , K + , Ca 2+ Mg 2+ , Cl - 、SO4 2- Plasma.

[0012] The organic pollutants include phenol, amide herbicides, neonicotinoid pesticides, etc. in water.

[0013] The beneficial effects of the present invention are as follows: the present invention utilizes a mixed solution of urea and an organic acid to pretreat eggshells, thereby breaking the dense calcium material structure of the eggshells; at the same time, urea amino groups form a weak binding force with eggshell calcium; a certain proportion of ferric pyrophosphate is added to obtain an eggshell calcium-iron complex; at the same time, urea increases the stability of the eggshell calcium-iron complex; after ultrasonic mixing, a certain proportion of a mixed organic acid solution of fumaric acid and citric acid is added; the mixture reacts under certain temperature conditions, so that the organic acid and the eggshell calcium-iron complex form an organic metal structure framework; and an eggshell calcium-based organic iron light-shielding salt-absorbing and pollution-reducing composite material is prepared; the composite material can absorb salt ions under non-light conditions and can effectively degrade organic pollutants, and can be used as a cheap environmental restoration material. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a picture showing the effect of eggshell calcium-based organic iron light-shielding composite material absorbing salt.

[0015] Figure 2 This is a diagram showing the effect of eggshell calcium-based organic iron light-shielding composite materials on degrading organic pollutants. DETAILED DESCRIPTION

[0016] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.

[0017] Example 1 Preparation of eggshell calcium-based organic iron light-shielding composite material and its salt absorption performance

[0018] 10.0 g of dried and crushed eggshells were added to 100 mL of a mixed solution containing urea, oxalic acid and prohexadione, wherein the amounts of urea, oxalic acid and prohexadione were 2.0 g, 0.1 g and 5.0 g, respectively. The mixture was ultrasonically treated for 5 min and reacted at 60 ° C for 5 h to obtain a calcium-based nitrogen-containing eggshell complex with a porous structure. 0.2 g of ferric pyrophosphate solid was added and ultrasonically treated for 3 min. The mixture was incubated on a constant temperature oscillator at 40 ° C and 180 r / min for 3 h to allow the iron ions to fully react with the eggshell. The calcium-based nitrogen-containing complex is bonded through urea amino hydrogen bonds; a mixed solid containing 1.0 g of fumaric acid and 0.5 g of citric acid is added in sequence, and ultrasonic treatment is performed for 3 minutes. The ultrasonic temperature is room temperature and the frequency is 20 kHz. The reaction is carried out at 80°C for 5 hours. After standing and cooling to room temperature, the solid-liquid separation is performed, and the mixture is washed three times with 50 mL of anhydrous ethanol and ultrapure water respectively. The separated solid is dried in a 60°C forced air drying oven for 8 hours, and then ground into powder to obtain the eggshell calcium-based organic iron light-shielding salt-absorbing and pollution-reducing composite material A1.

[0019] According to the above preparation method, the dosage of fumaric acid and citric acid was changed to 0.1g:0.5g and 0.2:0.5g respectively, and other reaction conditions and reaction processes remained unchanged, to obtain eggshell calcium-based organic iron light-shielding salt absorption and pollution reduction composite materials A2 and A3. The obtained composite material was fully mixed with an aqueous solution containing NaCl at a mass ratio of 1:100, and the original eggshell material was set as a control. The salt absorption reaction was carried out under illumination and non-illumination conditions for 5 hours, and the salt content in the water was measured. The results are shown in the attached Figure 1 As shown, overall, under light conditions, the salt absorption of the composite material ranges from 2 to 6 mg / g; under non-light conditions, the salt absorption of the composite material ranges from 25 to 32 mg / g, which is greater than the salt absorption of the composite material under light conditions, and when the dosage of fumaric acid and citric acid is 0.1g:0.5g, the maximum salt absorption of the composite material under non-light conditions is 32 mg / g.

[0020] Example 2 Effect of pretreatment time on the performance of eggshell calcium-based organic iron light-shielding composite materials

[0021] 10.0 g of dried and crushed eggshell was added to 100 mL of a mixed solution containing urea, oxalic acid and prohexadione, wherein the amounts of urea, oxalic acid and prohexadione were 2.0 g, 0.1 g and 5.0 g, respectively. The mixture was ultrasonically treated for 5 min and reacted at 60 ° C for 2 h to obtain a porous eggshell calcium-based nitrogen-containing complex. 0.2 g of ferric pyrophosphate solid was added and ultrasonically treated for 3 min. The ultrasonic temperature was room temperature, the frequency was 20 kHz, and the mixture was vibrated at a constant temperature of 40 ° C and 180 r / min. The mixture was cultured on an oscillator for 3 hours to allow the iron ions to fully bind to the eggshell calcium-based nitrogen-containing complex through urea amino hydrogen bonds; a mixed solid containing 0.1 g of fumaric acid and 0.5 g of citric acid was added in sequence, ultrasonically treated for 3 minutes, reacted at 80°C for 5 hours, allowed to stand and cool to room temperature, and then the solid-liquid was separated. The mixture was washed three times with 50 mL of anhydrous ethanol and ultrapure water respectively, and the separated solid was dried in a 60°C forced air drying oven for 8 hours, and then ground into powder to obtain an eggshell calcium-based organic iron light-shielding salt-absorbing and pollution-reducing composite material.

[0022] According to the above preparation method, the pretreatment time was changed to 3h and 4h respectively, and other reaction conditions and reaction processes remained unchanged, and the eggshell calcium-based organic iron light-shielding salt absorption and pollution reduction composite materials prepared under different pretreatment time conditions were obtained. The results showed that under non-light conditions, with the increase of pretreatment time, the salt absorption of the prepared eggshell calcium-based organic iron composite material increased from 18mg / g to 42mg / g. At the same time, under light conditions, the salt absorption of the eggshell calcium-based organic iron composite material prepared under three different pretreatment times was stable at 2-8mg / g, which further showed that the pretreatment time can further break the eggshell calcium dense structure, increase the proportion of eggshell calcium-based nitrogen-containing complexes, and thus improve the salt absorption performance of the eggshell calcium-based organic iron composite material.

[0023] Example 3 Effect of fumaric acid dosage on the performance of eggshell calcium-based organic iron light-shielding composite materials

[0024] 10.0 g of dried and crushed eggshell was added to 100 mL of a mixed solution containing urea, oxalic acid and prohexadione, wherein the amounts of urea, oxalic acid and prohexadione were 2.0 g, 0.1 g and 5.0 g, respectively. The mixture was ultrasonically treated for 5 min and reacted at 60 ° C for 4 h to obtain a porous eggshell calcium-based nitrogen-containing complex. 0.2 g of ferric pyrophosphate solid was added and ultrasonically treated for 3 min. The ultrasonic temperature was room temperature and the frequency was 20 kHz. The mixture was vibrated at a constant temperature of 40 ° C and 180 r / min. The mixture was cultured on an oscillator for 3 hours to allow the iron ions to fully bind to the eggshell calcium-based nitrogen-containing complex through urea amino hydrogen bonds; a mixed solid containing 1.0 g of fumaric acid and 0.5 g of citric acid was added in sequence, ultrasonically treated for 3 minutes, reacted at 80°C for 5 hours, allowed to stand and cool to room temperature, and then the solid-liquid was separated. The mixture was washed three times with 50 mL of anhydrous ethanol and ultrapure water respectively, and the separated solid was dried in a 60°C forced air drying oven for 8 hours, and then ground into powder to obtain an eggshell calcium-based organic iron light-shielding salt-absorbing and pollution-reducing composite material.

[0025] According to the above preparation method, the amount of fumaric acid was changed to 0.2g, 0.4g, 0.8g, and 1.0g respectively, and other reaction conditions and reaction processes remained unchanged, to obtain the eggshell calcium-based organic iron light-shielding salt absorption and pollution reduction composite material under different fumaric acid dosage conditions. The results showed that under non-illumination conditions, with the increase of fumaric acid dosage, the salt absorption of the prepared eggshell calcium-based organic iron composite material increased from 19mg / g to 51mg / g. At the same time, under illumination conditions, the salt absorption of the eggshell calcium-based organic iron composite material prepared under different fumaric acid dosage conditions did not change significantly. Therefore, as an organic iron ligand acid, increasing the amount of fumaric acid can increase the proportion of eggshell calcium-based organic iron composite material generation, thereby improving the salt absorption performance of the composite material.

[0026] Example 4 Preparation of eggshell calcium-based organic iron light-shielding composite material and its performance in degrading organic pollutants

[0027] 10.0 g of dried and crushed eggshell was added to 100 mL of a mixed solution containing urea, oxalic acid and prohexadione, wherein the amounts of urea, oxalic acid and prohexadione were 1.5 g, 1.0 g and 2.5 g, respectively. Ultrasonic treatment was performed for 5 min at room temperature and a frequency of 20 kHz. The reaction was performed at 60 ° C for 2 h to obtain a porous eggshell calcium-based nitrogen-containing complex. 0.5 g of ferric pyrophosphate solid was added and ultrasonic treatment was performed for 3 min. The mixture was oscillator was kept at 40 ° C and 180 r / min. The mixture was incubated for 4 hours to allow the iron ions to fully bind to the eggshell calcium-based nitrogen-containing complex through urea amino hydrogen bonds; a mixed solid containing 0.5 g of fumaric acid and 0.2 g of citric acid was added in sequence, ultrasonically treated for 3 minutes, reacted at 120°C for 3 hours, allowed to stand and cool to room temperature, and then the solid-liquid was separated. The mixture was washed three times with 50 mL of anhydrous ethanol and ultrapure water respectively, and the separated solid was dried in a 60°C forced air drying oven for 10 hours, and then ground into powder to obtain the eggshell calcium-based organic iron light-shielding salt-absorbing and pollution-reducing composite material B1.

[0028] According to the above preparation method, the reaction time after adding fumaric acid and citric acid mixed solids is 5h and 8h respectively, and other reaction conditions and reaction processes remain unchanged to obtain eggshell calcium-based organic iron light shielding salt absorption and pollution reduction composite materials B2 and B3. The obtained composite material is fully mixed with an aqueous solution containing phenol at a mass ratio of 1:100, the mass of the phenol aqueous solution is 50mL, and 0.05g of sodium persulfate is added in proportion. The original eggshell material is set as a control, and the degradation reaction is carried out under illumination and non-illumination conditions for 5h, respectively. The absorbance value of phenol in the water body is measured at 270nm by an ultraviolet spectrophotometer, and the removal rate of phenol in the water body is calculated. Overall, the removal rate of phenol in the water body by the eggshell raw material is 1.2% and 1.5% under illumination and non-illumination, respectively. The prepared composite material has a phenol removal rate of 12%-17% in water under illumination, while the composite material has a phenol removal rate of 95%-98% in water under non-illumination, and when the reaction time after adding the mixed solid of fumaric acid and citric acid is 5 hours, the composite material has a maximum phenol removal rate of 98% in water under non-illumination. Therefore, under non-illumination conditions, the composite material has a better ability to catalyze the degradation of phenol in water.

Claims

1. A method for preparing an eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material, characterized in that: Here are the steps: The dried eggshells are crushed to 40-100 meshes, and a mixed solution of urea, oxalic acid and prohexadione is added, wherein the mass ratio of the eggshell to the mixed solution is controlled to be 1:(10-20), and ultrasonic treatment is performed for 3-5 minutes, and the mixture is reacted at 50-60° C. for 2-5 hours to obtain an eggshell calcium-based nitrogen-containing complex having a porous structure; iron pyrophosphate of 1-5% of the mass of the eggshell is added to the eggshell calcium-based nitrogen-containing complex, and the mixture is ultrasonically treated for 3-5 minutes, and the mixture is cultured on a constant temperature oscillator at 40-50° C. and 180 r / min for 3-4 hours to allow the iron ions to fully react with the eggshell calcium. The nitrogen-containing complex is bonded by urea amino hydrogen bonds; then, fumaric acid and citric acid are added into a mixed solid in a ratio of 1%-10% and 1%-5% by weight of the eggshell, respectively, and ultrasonic treatment is performed for 3-5 minutes, the ultrasonic temperature is room temperature, the frequency is 20kHz, and the reaction is performed at 80-120°C for 3-8 hours. After standing and cooling to room temperature, the solid-liquid separation is performed, and the solid is washed three times in sequence with anhydrous ethanol and ultrapure water respectively. After the obtained solid is dried in a blast drying oven at 60°C for 8-10 hours, it is ground into powder to obtain the eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material.

2. The method according to claim 1, characterized in that The masses of the urea, oxalic acid and prohexadione are 1-2%, 0.1-1% and 2%-5% of the mass of the mixed aqueous solution respectively.

3. Application of the eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material obtained by the method of claim 1 or 2, characterized in that: The eggshell calcium-based organic iron light screen salt absorption and pollution reduction composite material is fully mixed with salt-containing or organic pollutant wastewater at a mass ratio of 1: (50-200). For organic pollutant wastewater, sodium persulfate needs to be additionally added at a ratio of 0.1%-0.5% of the wastewater mass. The reaction is carried out under non-light conditions for 5-10 hours, and the salt content or the amount of organic pollutants in the water body is regularly measured.

4. The use according to claim 3, characterized in that: The saline wastewater includes Na + , K + , Ca 2+ Mg 2+ , Cl - 、SO4 2- .

5. The use according to claim 3, characterized in that: The organic pollutants include phenol, amide herbicides and neonicotinoid insecticides in water.

Citation Information

Patent Citations

  • Preparation of straw / MIL-88A composite material and application of activated sodium persulfate in degradation of pesticides in soil

    CN113385233A

  • Ferric organic compounds, uses thereof and methods of making same

    CN1751056A