Modified nano MOF-5 filled PVA film and preparation method thereof
Through the preparation method of modified nano MOF-5 filled PVA film, the problems of poor mechanical properties and poor wear resistance of the modified PVA film coating are solved, and the wear resistance and mechanical properties of the composite coating are improved, and the preparation process is simplified. And reduces energy consumption.
Patent Information
- Application Number
- CN202411271699.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-29
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing modified PVA film coatings have poor mechanical properties and poor wear resistance in actual applications, which limits their wide application in the field of film coating materials.
Using modified nano MOF-5-filled PVA film preparation method, by dissolving Zn(NO3)2·6H2O and terephthalic acid in N,N-dimethylformamide, hexadecimal methyltetramine and H2O2 A white flocculent turbid liquid was formed, and the MOF-5 white powder material was obtained after centrifugation, washing and ultrasonic dispersion, and mixed with the PVA solution to prepare a MOF-5/PVA composite film.
Improve the wear resistance and mechanical properties of the composite coating, limit the size of MOF-5 particles by low temperature and hexadecimal methyltetramine and H2O2, improve the uniformity of dispersion in PVA, simplify the preparation process, and avoid the use of large-scale Equipment, low energy consumption.
Smart Images

Figure CN119081185A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal organic framework technology and thin film coating, and specifically relates to a PVA film filled with modified nano MOF-5 and a preparation method thereof. Background Art
[0002] Polyvinyl alcohol (PVA) has excellent film-forming properties, adhesive properties, biodegradability and good biocompatibility, and the thin film materials prepared from it have great application prospects. However, the side chain of polyvinyl alcohol contains many hydroxyl groups, which makes the film prepared from it insufficiently hydrophobic, thus affecting the mechanical properties and practical properties, which limits its wide application in the field of thin film coating materials. Therefore, the preparation of the corresponding nano-filled thin film coating will become a difficulty and breakthrough point in current research.
[0003] Nano-filling materials are the most critical factors affecting the performance of thin film coatings. Metal-Organic Frameworks (MOFs) can simultaneously have the adjustable size of organic molecules and the strength properties of inorganic materials. Therefore, it is of great significance to use MOFs materials as filling materials for thin films. However, the traditional method of modifying PVA thin film coatings mainly uses dicarboxylic acids (such as succinic acid) for cross-linking or inorganic substances (such as silica, titanium dioxide) as filling materials for modification. Among them, carboxylic acids have good compatibility with PVA, but as modified materials, their mechanical properties are still insufficient; although inorganic materials such as silica and titanium dioxide have higher mechanical properties, they seriously affect the color difference in the film and have poor abrasion resistance. Therefore, it is of great significance to explore a nano-MOFs-filled PVA film with both excellent mechanical properties and anti-friction properties. Summary of the invention
[0004] The purpose of the present invention is to provide a modified nano-MOF-5 filled PVA film and a preparation method thereof, so as to solve the problems of poor mechanical properties and poor wear resistance of existing modified PVA film coatings in practical applications.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a PVA film filled with modified nano MOF-5, comprising:
[0007] S1: dissolving Zn(NO3)2·6H2O and terephthalic acid in N,N-dimethylformamide to prepare solution A;
[0008] S2: Hexamethylenetetramine was added to solution A and stirred, and H2O2 was added dropwise during the stirring process to form a white flocculent turbid solution B;
[0009] S3: The white flocculent turbid liquid B is centrifuged to collect the solid powder, and the solid powder is washed alternately with DMF and chloroform, and then soaked in chloroform and dried to obtain the MOF-5 white powder material;
[0010] S4: Ultrasonic dispersion of the obtained MOF-5 white powder material in the PVA solution, stirring, and standing until there are no bubbles, to obtain a mixed solution C;
[0011] S5: Pour the mixed solution C onto a plate, scrape it flat, and let it stand and dry at room temperature to obtain a MOF-5 / PVA composite film.
[0012] Preferably, in S1, the content of Zn(NO3)2·6H2O is 0.90 g to 1.80 g, the content of terephthalic acid is 0.17 g to 0.50 g, and the content of N,N-dimethylformamide is 30 to 50 mL.
[0013] Preferably, in S1, Zn(NO3)2·6H2O and terephthalic acid are dissolved in N,N-dimethylformamide, stirred at room temperature for 10 minutes until clarified to obtain solution A, and solution A is placed in a refrigerator at 4°C for 2 hours until the solution temperature is constant.
[0014] Preferably, the content of hexamethylenetetramine in S2 is 50 mg to 100 mg, and the content of H2O2 is 0.1 to 0.2 mL.
[0015] Preferably, in S2, hexamethylenetetramine is added to solution A, and stirring is continued for 30 to 45 minutes in a cold water bath at 4° C., and H 2 O 2 is added dropwise during stirring.
[0016] Preferably, the white flocculent turbid liquid B in S3 is centrifuged at a speed of 8000 rpm, and the solid powder is washed alternately with DMF and chloroform for 10 times.
[0017] Preferably, the solid powder in S3 is soaked in 20 mL of chloroform for one day, the chloroform solution is changed every 6 hours, and finally vacuum dried at 99° C. for 12 hours.
[0018] Preferably, in S4, the MOF-5 white powder material is ultrasonically dispersed in a 12% PVA solution, stirred in a 50° C. water bath for 20 to 30 minutes, and then allowed to stand at room temperature for 12 hours to remove bubbles, to obtain a mixed solution C.
[0019] Preferably, in S5, the mixed solution C is poured onto a glass plate, flattened with a four-sided film applicator, and left to dry at room temperature.
[0020] A PVA film filled with modified nano-MOF-5, characterized in that it is prepared by any one of the preparation methods described above.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1) Utilize the mechanical properties of MOF-5 inorganic materials to improve the wear resistance and mechanical properties of the composite coating.
[0023] 2) Use low temperature, hexamethylenetetramine and H2O2 to jointly limit the particle size of MOF-5 and improve the uniformity of MOF-5 dispersion in PVA.
[0024] 3) Based on the principles of chemical thermodynamics and kinetics, chemical methods are used to regulate the synthesis of nano-MOF-5 and MOF-5 / PVA composite membranes, avoiding the use of large-scale instruments and equipment such as electrospinning. The method is simple, easy and has low energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 The XRD pattern of the MOF-5 / PVA composite film synthesized by the present invention;
[0027] Figure 2 This is a SEM photo of the MOF-5 / PVA composite film synthesized by the present invention;
[0028] Figure 3 is the stress-strain diagram of MOF-5 / PVA composite film;
[0029] Figure 4 This is a diagram showing the anti-friction performance of MOF-5 / PVA synthesized in the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0031] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0033] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0034] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0035] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0036] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0037] The present application discloses a method for preparing a PVA film filled with modified nano-MOF-5, comprising:
[0038] S1: dissolving Zn(NO3)2·6H2O and terephthalic acid in N,N-dimethylformamide to prepare solution A;
[0039] S2: Hexamethylenetetramine was added to solution A and stirred, and H2O2 was added dropwise during the stirring process to form a white flocculent turbid solution B;
[0040] S3: Centrifuge the white flocculent turbid liquid B to collect the solid powder, wash the solid powder alternately with DMF and chloroform, soak it in chloroform and dry it to obtain the MOF-5 white powder material;
[0041] S4: Ultrasonic dispersion of the obtained MOF-5 white powder material in the PVA solution, stirring, and standing until there are no bubbles, to obtain a mixed solution C;
[0042] S5: Pour the mixed solution C onto a plate, scrape it flat, and let it stand and dry at room temperature to obtain a MOF-5 / PVA composite film.
[0043] This application utilizes the mechanical properties of MOF-5 inorganic substances to improve the wear resistance and mechanical properties of the composite coating. Low temperature, hexamethylenetetramine, and H2O2 are used to jointly limit the particle size of MOF-5 and improve the uniformity of MOF-5 dispersion in PVA. Based on the principles of chemical thermodynamics and kinetics, chemical methods are used to regulate the synthesis of nano-MOF-5 and MOF-5 / PVA composite membranes, avoiding the use of large-scale instruments and equipment such as electrospinning. The method is simple, easy, and has low energy consumption.
[0044] In some embodiments, a method for preparing a PVA film filled with modified nano-MOF-5 comprises the following steps:
[0045] Step 1: Weigh 0.90 g to 1.80 g Zn(NO3)2·6H2O and 0.17 g to 0.50 g terephthalic acid, dissolve in 30 to 50 mL N,N-dimethylformamide, stir at room temperature for 10 minutes until clear, to prepare solution A, place solution A in a 4°C refrigerator for 2 hours until the solution temperature is constant.
[0046] Step 2: Weigh 50 mg to 100 mg of hexamethylenetetramine (HMTA), add it to solution A, and continue stirring in a cold water bath at 4°C for 30 to 45 minutes. During the stirring process, add 0.1 to 0.2 mL of H2O2 dropwise to form a white flocculent turbid solution B.
[0047] Step 3: Centrifuge the white flocculent turbid liquid B at 8000 rpm, collect the solid powder, wash it alternately with DMF and chloroform for 10 times, then soak it in 20 mL of chloroform for one day, change the chloroform solution every 6 hours, and finally dry it in vacuum at 99°C for 12 hours.
[0048] Step 4: Ultrasonic dispersion of the obtained MOF-5 white powder material in a 12% PVA solution was performed, and the mixture was stirred in a 50°C water bath for 20 to 30 minutes, and then allowed to stand at room temperature for 12 hours to remove bubbles, thereby obtaining a mixed solution C.
[0049] Step 5: Pour the mixed solution C onto a 5 cm × 2 cm glass plate, smooth it with a four-sided applicator, and let it stand and dry at room temperature for 24 hours to obtain a MOF-5 / PVA composite film.
[0050] Embodiment 1:
[0051] Step 1: Weigh 0.90 g of Zn(NO3)2·6H2O and 0.17 g of terephthalic acid, dissolve in 30 mL of N,N-dimethylformamide, and stir at room temperature for 10 minutes until it becomes clear to prepare solution A. Place solution A in a refrigerator at 4°C for 2 hours until the solution temperature remains constant.
[0052] Step 2: Weigh 50 mg of hexamethylenetetramine (HMTA) and add it to solution A. Stir continuously in a cold water bath at 4°C for 30 minutes. During the stirring process, add 0.1 mL of H2O2 dropwise to form a white flocculent turbid solution B.
[0053] Step 3: Centrifuge the white flocculent turbid liquid B at 8000 rpm, collect the solid powder, wash it alternately with DMF and chloroform for 10 times, then soak it in 20 mL of chloroform for one day, change the chloroform solution every 6 hours, and finally dry it in vacuum at 99°C for 12 hours.
[0054] Step 4: Ultrasonic dispersion of the obtained MOF-5 white powder material in a 12% PVA solution was performed, stirred in a 50°C water bath for 20 minutes, and then allowed to stand at room temperature for 12 hours to remove bubbles, to obtain a mixed solution C.
[0055] Step 5: Pour the mixed solution C onto a 5 cm × 2 cm glass plate, smooth it with a four-sided applicator, and let it stand and dry at room temperature for 24 hours to obtain a MOF-5 / PVA composite film.
[0056] Embodiment 2:
[0057] Step 1: Weigh 1.80 g Zn(NO3)2·6H2O and 0.50 g terephthalic acid, dissolve in 50 mL N,N-dimethylformamide, and stir at room temperature for 10 minutes until clear to prepare solution A. Place solution A in a refrigerator at 4°C for 2 hours until the solution temperature is constant.
[0058] Step 2: Weigh 100 mg of hexamethylenetetramine (HMTA) and add it to solution A. Stir continuously in a cold water bath at 4°C for 45 minutes. During the stirring process, add 0.2 mL of H2O2 dropwise to form a white flocculent turbid solution B.
[0059] Step 3: Centrifuge the white flocculent turbid liquid B at 8000 rpm, collect the solid powder, wash it alternately with DMF and chloroform for 10 times, then soak it in 20 mL of chloroform for one day, change the chloroform solution every 6 hours, and finally dry it in vacuum at 99°C for 12 hours.
[0060] Step 4: Ultrasonic dispersion of the obtained MOF-5 white powder material in a 12% PVA solution was performed, and the mixture was stirred for 30 minutes in a 50°C water bath, and then allowed to stand at room temperature for 12 hours to remove bubbles, thereby obtaining a mixed solution C.
[0061] Step 5: Pour the mixed solution C onto a 5 cm × 2 cm glass plate, flatten it with a four-sided applicator, and let it stand and dry at room temperature for 24 hours to obtain a MOF-5 / PVA composite film.
[0062] Embodiment 3:
[0063] Step 1: Weigh 1.5 g Zn(NO3)2·6H2O and 0.34 g terephthalic acid, dissolve in 40 mL N,N-dimethylformamide, and stir at room temperature for 10 minutes until clear to prepare solution A. Place solution A in a refrigerator at 4°C for 2 hours until the solution temperature is constant.
[0064] Step 2: Weigh 75 mg of hexamethylenetetramine (HMTA) and add it to solution A. Stir continuously in a cold water bath at 4°C for 40 minutes. During the stirring process, add 0.15 mL of H2O2 dropwise to form a white flocculent turbid solution B.
[0065] Step 3: Centrifuge the white flocculent turbid liquid B at 8000 rpm, collect the solid powder, wash it alternately with DMF and chloroform for 10 times, then soak it in 20 mL of chloroform for one day, change the chloroform solution every 6 hours, and finally dry it in vacuum at 99°C for 12 hours.
[0066] Step 4: Ultrasonic dispersion of the obtained MOF-5 white powder material in a 12% PVA solution was performed, stirred for 25 minutes in a 50°C water bath, and then allowed to stand at room temperature for 12 hours to remove bubbles, to obtain a mixed solution C.
[0067] Step 5: Pour the mixed solution C onto a 5 cm × 2 cm glass plate, smooth it with a four-sided applicator, and let it stand and dry at room temperature for 24 hours to obtain a MOF-5 / PVA composite film.
[0068] Embodiment 4:
[0069] Step 1: Use a servo material multifunctional high and low temperature tensile machine to test the tensile properties of the MOF-5 / PVA composite film. First, cut the film into a width of 1 cm and a length of 5 cm. The sample surface should be flat and smooth, with no cracks on the edges and no bubbles inside. Then test the tensile strength of the film at a speed of 10 mm / min. Prepare 5 parallel samples and take the average value after testing.
[0070] Step 2: Use a multifunctional friction and wear tester to measure the friction coefficient and time of the MOF-5 / PVA composite film. The MOF-5 / PVA composite film is attached to the stainless steel substrate with double-sided tape, the upper sample is a GCr15 steel ball, the experimental load is 100g, the test time is 30min, the rotation speed is 200r / min, and each group of specimens is measured three times to take the average value.
[0071] See also Figure 1 , MOF-5 / PVA composite film has characteristic peaks of PVA and MOF-5, indicating that the two are successfully composited.
[0072] See also Figure 2 The MOF-5 nanoparticles are evenly distributed on the surface of the MOF-5 / PVA composite film, forming a relatively rough surface, which promotes the improvement of friction resistance.
[0073] See also Figure 3 , the tensile strength of the MOF-5 / PVA composite film can be increased to 60MPa, which is about 3 times that of the pure PVA film.
[0074] See also Figure 4 The friction coefficient of MOF-5 / PVA composite film is less than 0.1, and it is wirelessly smooth and has good stability, which is better than the performance of pure PVA film.
[0075] In summary, the present invention discloses a PVA film filled with modified nano MOF-5 and a preparation method, which belongs to the field of high-performance composite thin film coatings. In the present invention, the mechanical properties of the inorganic MOF-5 are used to improve the wear resistance and mechanical properties of the composite coating. The particle size of MOF-5 is limited by low temperature, hexamethylenetetramine, and H2O2 to improve the uniformity of MOF-5 dispersion in PVA. Based on the principles of chemical thermodynamics and kinetics, chemical methods are used to regulate the synthesis of nano MOF-5 and MOF-5 / PVA composite films, avoiding the use of large-scale instruments and equipment such as electrospinning. The method is simple, easy to operate, and has low energy consumption.
[0076] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a PVA film filled with modified nano-MOF-5, characterized in that: include: S1: dissolving Zn(NO3)2·6H2O and terephthalic acid in N,N-dimethylformamide to prepare solution A; S2: Hexamethylenetetramine was added to solution A and stirred, and H2O2 was added dropwise during the stirring process to form a white flocculent turbid solution B; S3: The white flocculent turbid liquid B is centrifuged to collect the solid powder, and the solid powder is washed alternately with DMF and chloroform, and then soaked in chloroform and dried to obtain the MOF-5 white powder material; S4: Ultrasonic dispersion of the obtained MOF-5 white powder material in the PVA solution, stirring, and standing until there are no bubbles, to obtain a mixed solution C; S5: Pour the mixed solution C onto a plate, scrape it flat, and let it stand and dry at room temperature to obtain a MOF-5 / PVA composite film.
2. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: In the S1, the content of Zn(NO3)2·6H2O is 0.90g-1.80g, the content of terephthalic acid is 0.17g-0.50g, and the content of N,N-dimethylformamide is 30-50mL.
3. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: In the S1, Zn(NO3)2·6H2O and terephthalic acid are dissolved in N,N-dimethylformamide and stirred at room temperature for 10 minutes until it becomes clear to obtain solution A. Solution A is placed in a refrigerator at 4°C for 2 hours until the solution temperature is constant.
4. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: The hexamethylenetetramine in the S2 is 50 mg to 100 mg, and the H2O2 is 0.1 to 0.2 mL.
5. The method for preparing a modified nano-MOF-5 filled PVA film according to claim 1, characterized in that: In the S2, hexamethylenetetramine is added to solution A, and stirring is continued for 30 to 45 minutes in a cold water bath at 4°C, and H2O2 is added dropwise during stirring.
6. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: The white flocculent turbid liquid B in the S3 was centrifuged at a speed of 8000 rpm, and the solid powder was washed alternately with DMF and chloroform for 10 times.
7. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: The solid powder in S3 was soaked in 20 mL of chloroform for one day, the chloroform solution was changed every 6 hours, and finally vacuum dried at 99° C. for 12 hours.
8. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: In the S4, the MOF-5 white powder material is ultrasonically dispersed in a PVA solution with a concentration of 12%, stirred in a 50° C. water bath for 20 to 30 minutes, and then allowed to stand at room temperature for 12 hours to remove bubbles, thereby obtaining a mixed solution C.
9. The method for preparing a PVA film filled with modified nano-MOF-5 according to claim 1, characterized in that: In the above S5, the mixed solution C is poured onto a glass plate, flattened with a four-sided film applicator, and left to dry at room temperature.
10. A PVA film filled with modified nano-MOF-5, characterized in that: The method is prepared by any one of claims 1 to 9.
Citation Information
Patent Citations
Parallelepiped zinc oxide aggregate and preparation method thereof
CN103991897A
ZIF-8 / poly(vinyl alcohol) (PVA) composite nanofiber membrane as well as preparation method and application thereof
CN105951304A
Preparation method of copper metal organic frameworks / polyvinyl alcohol nanocomposite films