Polypropylene composite material as well as preparation method and application thereof
Through a twin-screw extrusion process combining polypropylene resin with inorganic fillers, tougheners, glass slag, etc., a polypropylene composite material with high gloss and excellent mechanical properties was prepared, which solved the poor dimensional stability and spraying of existing polypropylene materials. The complex process has achieved lightweight and environmentally friendly production of automotive parts.
Patent Information
- Application Number
- CN202411342821.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The existing polypropylene composite materials have poor dimensional stability in automotive exterior parts, cannot meet the high dimensional requirements, and the spraying process is complex, resulting in waste of resources and environmental pollution.
Using a combination of polypropylene resin, inorganic filler, toughener, glass slag, masterbatch and additive, melt-kneaded through a twin-screw extruder to prepare a polypropylene composite material with high gloss and good dimensional stability. , used to replace metal materials, reduce spraying, reduce costs and environmental impact.
It has achieved high gloss and excellent mechanical properties of polypropylene composite materials, improved dimensional stability, and high gloss of the material itself, which can replace metals for automotive parts, reduce weight, reduce resource waste and environmental pollution, and is suitable for automotive lightweight, Comfortable and safe development.
Smart Images

Figure BDA0005060186900000041 
Figure BDA0005060186900000051 
Figure BDA0005060186900000052
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to a polypropylene composite material and a preparation method and application thereof. Background Art
[0002] During the automobile manufacturing process, for exterior decorative parts such as bumpers and wheel eyebrows, plastic substrates are usually spray-painted. The surface decorative paint can not only protect the resin substrate, but also achieve surface effects such as high gloss and matte, as well as functions such as weather resistance and scratch resistance. However, the spraying process is complicated. After the injection molding of the blank parts, it is necessary to add basic links such as transportation, pretreatment, painting, and transportation. Some spraying processes also need to go through multiple production processes such as primer, topcoat, and UV curing paint. In addition, for defective parts in the production process, since thermosetting paint has been sprayed and cannot be easily peeled off, it is difficult to recycle, wastes resources, and pollutes the environment. If the raw materials used to prepare automotive parts have high gloss characteristics, the parts can have their own gloss, thereby eliminating the spraying process, balancing the quality of the parts and the preparation cost, while being more environmentally friendly.
[0003] Polypropylene composite materials have the characteristics of low density and low price, and are widely used in the preparation of automotive parts. However, parts such as fenders and tailgates in automotive exteriors need to match the size of multiple surrounding parts, and the dimensional stability requirements of the products are very strict. Therefore, these parts are currently mainly made of metal, with heavy product weight and low design freedom. Although using polypropylene composite materials instead of metal in the preparation of such parts can greatly reduce the weight of parts and achieve the purpose of lightweighting, conforming to the development trend of lightweight, comfortable and safe automobiles, ordinary polypropylene materials have the defects of large shrinkage and poor dimensional stability, and cannot meet the high dimensional stability requirements of parts. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a polypropylene composite material; the second purpose of the present invention is to provide a method for preparing the polypropylene composite material; the third purpose of the present invention is to provide an application of the polypropylene composite material.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides a polypropylene composite material, comprising the following preparation raw materials: polypropylene resin, inorganic filler, toughening agent, glass slag, masterbatch, and additives.
[0007] Preferably, the polypropylene composite material comprises the following raw materials in mass percentage: 50-70% polypropylene resin, 5-25% inorganic filler, 1-20% toughening agent, 1-10% glass slag, 0.1-1% masterbatch, and 0.2-2% additive; further preferably, the polypropylene composite material comprises the following raw materials in mass percentage: 60-70% polypropylene resin, 10-20% inorganic filler, 5-15% toughening agent, 2-8% glass slag, 0.5-1% masterbatch, and 0.2-1% additive.
[0008] Preferably, the glossiness of the polypropylene resin at 60° is ≥80%; further preferably, the glossiness of the polypropylene resin at 60° is 85-95%.
[0009] Preferably, the melt index of the polypropylene resin under the test condition of 230°C / 2.16kg is 1g / 10min-100g / 10min; further preferably, the melt index of the polypropylene resin under the test condition of 230°C / 2.16kg is 20g / 10min-30g / 10minn.
[0010] Preferably, the polypropylene resin includes at least one of homopolymer polypropylene and block copolymer polypropylene; further preferably, the polypropylene resin is PP EP548G of China SABIC (Tianjin) Petrochemical Co., Ltd. This PP raw material is polymerized using the Spherizone process, and by adjusting the ethylene content, controlling the rubber phase content and size, etc., it achieves a glossiness 25% higher than that of ordinary copolymer PP raw materials.
[0011] Preferably, the particle size of the inorganic filler is 0.5-10 μm; more preferably, the particle size of the inorganic filler is 1-3 μm.
[0012] Preferably, the inorganic filler includes at least one of barium sulfate and wollastonite; further preferably, the inorganic filler is barium sulfate.
[0013] Preferably, the melt index of the toughening agent under the test condition of 190°C / 2.16kg is 10g / 10min-30g / 10min; further preferably, the melt index of the toughening agent under the test condition of 190°C / 2.16kg is 13g / 10min-30g / 10min.
[0014] Preferably, the toughening agent includes at least one of ethylene-propylene rubber, ethylene-octene copolymer, ethylene-butene copolymer, and ethylene-vinyl acetate copolymer; further preferably, the toughening agent is ethylene-octene copolymer (POE).
[0015] Specifically, when the elastomer POE is used as a toughening agent, the elastomer itself has a negative effect on the gloss of the polypropylene composite material, but the elastomer with a relatively high melt index (190°C / 2.16kg, 10g / 10min-30g / 10min) is more easily stretched into strips in the polypropylene resin matrix, thereby reducing the adverse effect of the toughening agent on the gloss of the material while enhancing the mechanical properties of the material.
[0016] Preferably, the glass slag has a flaky structure; the thickness-to-diameter ratio of the glass slag is 1:(10-50); further preferably, the thickness-to-diameter ratio of the glass slag is 1:(15-25).
[0017] Specifically, by introducing special glass slag fillers into the formula system, the glass slag with a certain size and a flaky structure has a good light radiation effect and can provide better gloss for the polypropylene composite material; and the flaky structure of the glass slag can hinder the crystallization of the polypropylene matrix resin, thereby reducing the linear expansion coefficient of the polypropylene composite material and improving the dimensional stability of the material.
[0018] Preferably, the carbon black content of the masterbatch is 20-60wt%; further preferably, the carbon black content of the masterbatch is 30-50wt%.
[0019] Preferably, the masterbatch is a PP resin carrier.
[0020] Preferably, the auxiliary agent includes an antioxidant and a lubricant.
[0021] Preferably, the mass ratio of the antioxidant to the lubricant is (1-1.5):1; further preferably, the mass ratio of the antioxidant to the lubricant is (1.2-1.5):1.
[0022] Preferably, the antioxidant includes at least one of a hindered phenol antioxidant, a thioester antioxidant, and a phosphite antioxidant; further preferably, the antioxidant is a composite antioxidant of a hindered phenol antioxidant and a phosphite antioxidant.
[0023] Preferably, the mass ratio of the hindered phenol antioxidant to the phosphite antioxidant is 1:(1-2); further preferably, the mass ratio of the hindered phenol antioxidant to the phosphite antioxidant is 1:(1.5-2).
[0024] Preferably, the hindered phenol antioxidant includes at least one of 2,6-di-tert-butyl-p-methylphenol (BHT), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076), pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1010), N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl) hexanediamine (antioxidant 1098), and triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate] (antioxidant 245); further preferably, the hindered phenol antioxidant is antioxidant 1010.
[0025] Preferably, the phosphite antioxidant includes at least one of diphenyl isooctyl phosphite (ODPP), tris[2.4-di-tert-butylphenyl]phosphite (antioxidant 168), bisphenol A phosphite, and triphenyl phosphite (TPP); further preferably, the phosphite antioxidant is antioxidant 168.
[0026] Preferably, the lubricant includes at least one of stearate and silicone masterbatch; further preferably, the lubricant is stearate.
[0027] The second aspect of the present invention provides a method for preparing the polypropylene composite material according to the first aspect of the present invention, comprising the following steps:
[0028] S1, first mix the polypropylene resin, inorganic filler and toughening agent, then add the masterbatch and additives and mix well to obtain a premix;
[0029] S2. Adding glass slag to the premix, performing melt mixing through a twin-screw extruder, and extruding and granulating to obtain the polypropylene composite material.
[0030] Preferably, in step S1, the premix is mixed at a speed of 800-1500 r / min for 5-10 min.
[0031] Preferably, in step S2, the temperatures of the feeding sections of the twin-screw extruder are set to 160-165°C, 160-165°C, 160-165°C, 160-165°C, 160-170°C, 170-180°C, 180-190°C, 190-200°C, 200-210°C, the head temperature is 200-210°C, and the screw speed is 300-600r / min.
[0032] Preferably, in step S2, the screw assembly of the twin-screw extruder comprises a toothed disc thread element.
[0033] The third aspect of the present invention provides use of the polypropylene composite material described in the first aspect of the present invention in the preparation of automotive interior and exterior parts.
[0034] Preferably, the automobile interior and exterior parts include fenders and tailgates.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The polypropylene composite material provided by the present invention has a glossiness of more than 90% at 60° and a linear expansion coefficient of less than 50×10 -6 / K, the material size changes little with temperature and has good dimensional stability; the material has excellent mechanical properties.
[0037] (2) The preparation method of the polypropylene composite material provided by the present invention is simple, the process conditions are mild, and it is suitable for industrial application.
[0038] (3) The polypropylene composite material provided by the present invention has high gloss. When used to prepare automotive interior and exterior parts, the spraying process can be eliminated, which reduces costs and is environmentally friendly. The material has good dimensional stability and good mechanical properties. It can replace metal in the preparation of vehicle fenders and tailgates and other parts, conforming to the development trend of lightweight, comfortable and safe automobiles. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0040] The raw material information used in the following examples and comparative examples is shown in Table 1 below:
[0041] Table 1 Information of raw materials used in the examples and comparative examples
[0042]
[0043] Among them, the melting index of polypropylene resin PP EP548G under the test condition of 230℃ / 2.16kg is 26g / 10min, PP EP548G is a high-gloss resin with a glossiness ≥80% at 60°; the melting index of PP EP548R under the test condition of 230℃ / 2.16kg is 26g / 10min, which is a common gloss resin; the melting index of toughener POE8613 under the test condition of 190℃ / 2.16kg is 13g / 10min; the melting index of POE565 under the test condition of 190℃ / 2.16kg is 5g / 10min; the carbon black content of masterbatch Cabot XP6622A is 40wt%; the particle size of barium sulfate LC-330 is 1.5μm.
[0044] Example 1
[0045] This example prepares a polypropylene composite material, and the raw materials are shown in Table 2:
[0046] Table 2 Example 1 Polypropylene composite material raw material composition
[0047]
[0048] The preparation method of the polypropylene composite material comprises the following steps:
[0049] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0050] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0051] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, adding glass slag from the side feeding port, and melt-extruding and granulating to obtain a polypropylene composite material.
[0052] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0053] Example 2
[0054] This example prepares a polypropylene composite material, and the raw materials are shown in Table 3:
[0055] Table 3 Example 2 Polypropylene composite material raw material composition
[0056]
[0057]
[0058] The preparation method of the polypropylene composite material comprises the following steps:
[0059] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0060] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0061] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, adding glass slag from the side feeding port, and melt-extruding and granulating to obtain a polypropylene composite material.
[0062] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0063] Example 3
[0064] This example prepares a polypropylene composite material, and the raw materials are shown in Table 4:
[0065] Table 4 Example 3 Polypropylene composite material raw material composition
[0066]
[0067] The preparation method of the polypropylene composite material comprises the following steps:
[0068] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0069] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0070] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, adding glass slag from the side feeding port, and melt-extruding and granulating to obtain a polypropylene composite material.
[0071] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0072] Example 4
[0073] This example prepares a polypropylene composite material, and the raw materials are shown in Table 5:
[0074] Table 5 Example 4 Polypropylene composite material raw material composition
[0075]
[0076] The preparation method of the polypropylene composite material comprises the following steps:
[0077] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0078] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0079] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, adding glass slag from the side feeding port, and melt-extruding and granulating to obtain a polypropylene composite material.
[0080] Among them, the screw combination of the twin-screw extruder has added toothed disc thread components. The temperatures of each feeding section are set to 160℃, 160℃, 160℃, 160℃, 165℃, 170℃, 180℃, 190℃, and 200℃. The head temperature is 210℃ and the screw speed is 500r / min.
[0081] Example 5
[0082] This example prepares a polypropylene composite material, and the raw materials are shown in Table 6:
[0083] Table 6 Example 5 Polypropylene composite material raw material composition
[0084]
[0085] The preparation method of the polypropylene composite material comprises the following steps:
[0086] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0087] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0088] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, adding glass slag from the side feeding port, and melt-extruding and granulating to obtain a polypropylene composite material.
[0089] Among them, the screw combination of the twin-screw extruder has added toothed disc thread components. The temperatures of each feeding section are set to 160℃, 160℃, 160℃, 160℃, 165℃, 170℃, 180℃, 190℃, and 200℃. The head temperature is 210℃ and the screw speed is 500r / min.
[0090] Comparative Example 1
[0091] This comparative example prepares a polypropylene composite material, and the raw materials are shown in Table 7:
[0092] Table 7 Comparative Example 1 Polypropylene composite material raw material composition
[0093]
[0094]
[0095] The preparation method of the polypropylene composite material comprises the following steps:
[0096] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0097] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0098] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, and melt-extruding and granulating to obtain a polypropylene composite material.
[0099] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0100] Comparative Example 2
[0101] This comparative example prepares a polypropylene composite material, and the raw materials are shown in Table 8:
[0102] Table 8 Comparative Example 2 Polypropylene Composite Material Raw Material Composition
[0103]
[0104] The preparation method of the polypropylene composite material comprises the following steps:
[0105] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0106] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0107] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, and melt-extruding and granulating to obtain a polypropylene composite material.
[0108] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0109] Comparative Example 3
[0110] This comparative example prepares a polypropylene composite material, and the raw materials are shown in Table 9:
[0111] Table 9 Comparative Example 3 Polypropylene Composite Material Raw Material Composition
[0112]
[0113] The preparation method of the polypropylene composite material comprises the following steps:
[0114] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0115] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0116] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, and melt-extruding and granulating to obtain a polypropylene composite material.
[0117] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0118] Comparative Example 4
[0119] This comparative example prepares a polypropylene composite material, and the raw materials are shown in Table 10:
[0120] Table 10 Comparative Example 4 Polypropylene Composite Material Raw Material Composition
[0121]
[0122]
[0123] The preparation method of the polypropylene composite material comprises the following steps:
[0124] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0125] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0126] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, and melt-extruding and granulating to obtain a polypropylene composite material.
[0127] Among them, the screw combination of the twin-screw extruder has added toothed disc thread components. The temperatures of each feeding section are set to 160℃, 160℃, 160℃, 160℃, 165℃, 170℃, 180℃, 190℃, and 200℃. The head temperature is 210℃ and the screw speed is 500r / min.
[0128] Comparative Example 5
[0129] This comparative example prepares a polypropylene composite material, and the raw materials are shown in Table 11:
[0130] Table 11 Comparative Example 5 Polypropylene Composite Material Raw Material Composition
[0131]
[0132] The preparation method of the polypropylene composite material comprises the following steps:
[0133] S1, mixing polypropylene resin, inorganic filler and toughening agent, adding antioxidant, lubricant and masterbatch and continuing to mix evenly to obtain a premix;
[0134] S2, mixing the premix at a speed of 1200 r / min for 10 min;
[0135] S3, adding the mixed premix from the main feeding port of the twin-screw extruder, and melt-extruding and granulating to obtain a polypropylene composite material.
[0136] Among them, the temperatures of each feeding section of the twin-screw extruder were set to 160°C, 160°C, 160°C, 160°C, 165°C, 170°C, 180°C, 190°C, and 200°C, the head temperature was 210°C, and the screw speed was 500r / min.
[0137] Performance Testing
[0138] The gloss (60°), linear expansion coefficient, tensile strength, elongation at break, impact strength and shrinkage of the polypropylene composite materials in Examples 1-5 and Comparative Examples 1-5 were tested. The test methods and standards are shown in Table 12, and the test results are shown in Table 13.
[0139] Table 12 Reference standards for performance test of polypropylene composite materials
[0140] Test items Reference Standards Gloss (60°) Plastic gloss standard GB / T8807-1998 Linear expansion coefficient ISO11359-1, temperature range is -30-100℃ Tensile Strength ISO 527-1-2012 Elongation at break ISO 527-1-2012 Impact strength ISO 180-2000 Shrinkage ISO 294-4-2001
[0141] Table 13 Test results of polypropylene composite materials in Examples 1-5 and Comparative Examples 1-5
[0142]
[0143]
[0144] Table 13 shows the test results of the polypropylene composite materials in Examples 1-5 and Comparative Examples 1-5. It can be seen from Table 13 that the polypropylene composite materials prepared in Examples 1-5 using high gloss polypropylene resin as the resin matrix, barium sulfate as the inorganic filler, POE elastomer with a melt index of 13 g / 10 min at 190°C / 2.16 kg as the toughening agent, and glass slag as the addition have a high gloss (60°) that can reach more than 90%, and the linear expansion coefficient of the material in the temperature range of -30-100°C can be as low as 50×10 -6 / K or less, indicating that the material size changes little with temperature and has high dimensional stability; the material's tensile strength can reach 22MPa, the elongation at break is high, reaching 270%, and the impact strength can reach 37KJ / m 2 The shrinkage rate can reach below 0.9%, indicating that the material has excellent mechanical properties, is not easy to break, has excellent deformation and impact resistance, and has high quality and reliability.
[0145] Compared with Example 3 and Example 4, the raw material composition of the material is the same, but when preparing the polypropylene composite material in Example 4, the screw assembly of the twin-screw extruder used adds a toothed disc thread element, and it can be seen that the gloss and mechanical properties of the material in Example 4 are improved. It shows that compared with ordinary shear dispersion thread elements, the toothed disc thread element can better disperse the toughening agent and inorganic filler, thereby optimizing the mechanical properties of the material; and the toothed disc thread element has a smaller degree of damage to the sheet structure of the glass slag, so that the glass slag can better maintain the sheet structure, thereby having better light radiation ability and improving the gloss of the material.
[0146] Compared with Example 4, Example 5 uses glass slag with a larger aspect ratio, and the glossiness of the material is further improved, indicating that glass slag with a larger aspect ratio has a stronger light radiation ability and is more conducive to improving the glossiness of the material.
[0147] In Comparative Example 1, ordinary glossy polypropylene resin is used as the resin matrix, talcum powder is used as the inorganic filler, and elastomer POE with a melt index of 5g / 10min at 190℃ / 2.16kg is used as the toughening agent. No glass slag is added to prepare a polypropylene composite material. It can be seen that the glossiness of the polypropylene composite material in Comparative Example 1 at 60° is only 54%, which is low in glossiness; the linear expansion coefficient is as high as 81×10 -6 / K, poor dimensional stability; low tensile strength, elongation at break and impact strength, high shrinkage, and poor overall mechanical properties of the material.
[0148] Compared with Comparative Example 1, Comparative Example 2 replaces the resin matrix with high-gloss polypropylene resin. It can be seen that the mechanical properties of the material do not change much, but the glossiness is improved, indicating that using high-gloss polypropylene resin as raw material has a positive effect on improving the glossiness of polypropylene composite materials.
[0149] Comparative Example 3 Compared with Comparative Example 2, the low melt index elastomer POE565 is replaced by the high melt index elastomer POE8613. It can be seen that the mechanical properties of the material are improved, the dimensional stability is improved, and the gloss is not affected. The elastomer itself has a negative impact on the gloss of the polypropylene composite material, but the present invention uses a high melt index elastomer with a melt index of 10g / 10min-30g / 10min under the test conditions of 190°C / 2.16kg. The high melt index elastomer is relatively easier to be stretched into strips in the polypropylene resin matrix, so that it improves the mechanical properties of the material while having less effect on the gloss of the polypropylene composite material.
[0150] Compared with Comparative Example 3, the raw material composition of the materials in Comparative Example 4 is the same, but when preparing the polypropylene composite material, the screw assembly of the twin-screw extruder used in Comparative Example 4 adds a toothed disc thread element, and it can be seen that the glossiness and mechanical properties of the material are improved. This shows that compared with ordinary shear dispersion thread elements, the toothed disc thread element can better disperse the toughening agent and the inorganic filler, thereby optimizing the mechanical properties of the material.
[0151] Compared with Comparative Example 3, in Comparative Example 5, the inorganic filler talc powder is replaced with barium sulfate, and it can be seen that the glossiness of the material is improved.
[0152] The polypropylene composite material provided by the present invention uses polypropylene resin with high gloss as a base material to lay a foundation for the high gloss of the material, and then adds glass slag with a flaky structure to optimize the gloss of the composite material by utilizing its light radiation effect; at the same time, the glass slag can also hinder the crystallization of the base resin, thereby improving the dimensional stability of the material; a toughening agent with a high melt index is used to make it easier to be stretched into strips in the base material, thereby reducing the influence of the toughening agent on the gloss of the material while improving the mechanical properties of the material; by adding additives such as antioxidants and lubricants, the weather resistance and processing performance of the material are improved, and finally a polypropylene composite material with high gloss, good dimensional stability and excellent mechanical properties is obtained, and the preparation method of the material is simple and can meet the application requirements of preparing automotive interior and exterior parts.
Claims
1. A polypropylene composite material, It is characterized in that The preparation comprises the following raw materials: polypropylene resin, inorganic filler, toughening agent, glass slag, masterbatch and additives.
2. The polypropylene composite material according to claim 1, It is characterized in that The polypropylene composite material comprises the following raw materials in percentage by mass: 50-70% of polypropylene resin, 5-25% of inorganic filler, 1-20% of toughening agent, 1-10% of glass slag, 0.1-1% of masterbatch and 0.2-2% of auxiliary agent.
3. The polypropylene composite material according to claim 1, It is characterized in that The glossiness of the polypropylene resin at 60° is ≥80%; And / or, the polypropylene resin has a melt index of 1 g / 10 min-100 g / 10 min under the test condition of 230° C. / 2.16 kg.
4. The polypropylene composite material according to claim 1, It is characterized in that The particle size of the inorganic filler is 0.5-10 μm; Preferably, the inorganic filler includes at least one of barium sulfate and wollastonite.
5. The polypropylene composite material according to claim 1, It is characterized in that The melt index of the toughening agent under the test condition of 190°C / 2.16kg is 10g / 10min-30g / 10min; Preferably, the toughening agent includes at least one of ethylene-propylene rubber, ethylene-octene copolymer, ethylene-butene copolymer, and ethylene-vinyl acetate copolymer.
6. The polypropylene composite material according to claim 1, It is characterized in that The glass slag has a flaky structure; the thickness-to-diameter ratio of the glass slag is 1:(10-50).
7. The polypropylene composite material according to claim 1, It is characterized in that The carbon black content of the masterbatch is 20-60wt%.
8. The polypropylene composite material according to claim 1, It is characterized in that The auxiliary agents include antioxidants and lubricants; And / or, the mass ratio of the antioxidant to the lubricant is (1-1.5):
1.
9. A method for preparing the polypropylene composite material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1, first mix the polypropylene resin, inorganic filler and toughening agent, then add the masterbatch and additives and mix well to obtain a premix; S2. Adding glass slag to the premix, performing melt mixing through a twin-screw extruder, and extruding and granulating to obtain the polypropylene composite material.
10. Use of the polypropylene composite material according to any one of claims 1 to 8 in the preparation of automotive interior and exterior parts.
Citation Information
Patent Citations
High-rigidity, low-shrinkage and good-appearance polypropylene composite material and preparation method thereof
CN105602179A
High-gloss, precipitation-resistant and low-warping enhanced halogen-free flame-retardant polypropylene and preparation method thereof
CN109749243A
Flat glass fiber reinforced flame-retardant PP composite material and preparation method thereof
CN111808365A
Low-floating-fiber flame-retardant polypropylene material
CN115403890A
Flexible polypropylene composite material and its molded product
JP2005015558A
Cited By
High-performance polypropylene plastic bucket material and preparation method thereof
CN121517820A