Novel rubber compound and preparation method thereof
By using organically modified montmorillonite and peroxide vulcanization systems in rubber kneading glue, combining white hydrogenated paraffin oil and adsorbent deodorant, the rubber kneading glue in the prior art has been solved by slow vulcanization speed, large odor and resistant to rubber kneading glue in the prior art. The problem of poor thermal performance achieves rapid vulcanization, low odor and high heat resistance, and simplifies the preparation process, which is suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202410990012.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-12-06
AI Technical Summary
When the existing rubber mixing glue increases the vulcanization speed, it will cause odor to worsen and reduce heat resistance. The preparation method is complex and inefficient, making it difficult to meet the requirements of rapid vulcanization, low odor, high heat resistance and low compression permanent deformation.
Using new rubber mixed rubber formulas, including raw rubber, reinforcement, filler, deodorant, anti-aging agent and specific vulcanizing agent, through organically modified montmorillonite and peroxide vulcanization system, combined with pharmacopoeia grade white hydrogenated paraffin wax Oil and adsorbent deodorants achieve rapid vulcanization and high heat resistance, while reducing odor and compression permanent deformation through reasonable process steps and temperature control.
It realizes the comprehensive performance of rapid vulcanization, low odor, high heat resistance and low compression permanent deformation, simplifies the preparation process, improves industrial production efficiency, and is suitable for a variety of application scenarios.
Smart Images

Figure BDA0004958600030000061 
Figure BDA0004958600030000071 
Figure BDA0004958600030000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber compounding, and in particular to a novel rubber compounding and a preparation process thereof. Background Art
[0002] Rubber materials are widely used in daily life, industrial production and high-tech fields due to their excellent elasticity, insulation, chemical stability, oil resistance, flame resistance and other properties. However, in different fields of application, rubber materials need to meet different specific requirements, such as fast vulcanization, low odor, high heat resistance and low compression set.
[0003] In the existing technology, increasing the vulcanization speed of rubber mix is usually achieved by adding more vulcanizing agent. However, this will cause the odor of the rubber mix to increase and may reduce its heat resistance. In addition, the existing preparation methods usually involve complicated process steps and harsh operating conditions, which are inefficient and difficult to achieve large-scale production for industrial production.
[0004] In addition, the permanent deformation performance of existing rubber compounds is often unsatisfactory when subjected to compression, which limits its application range. Therefore, it is of great practical application value to develop a rubber compound and a preparation method thereof that can simultaneously meet the requirements of rapid vulcanization, low odor, high heat resistance and low compression permanent deformation and has a simple preparation method. Summary of the invention
[0005] The technical problem to be solved by the present invention is: in order to overcome the above disadvantages, a new type of rubber compound with fast vulcanization speed, low odor, high heat resistance and low compression permanent deformation and a preparation method thereof are provided. The rubber compound of the present invention is mainly composed of rubber raw materials, vulcanizing agents, accelerators, heat-resistant agents and deodorants, etc. The unique properties of each component and the reasonable ratio make the rubber compound have good comprehensive properties.
[0006] The technical solution is: a new type of rubber compound, including the following components in parts by weight (PHR):
[0007] Raw rubber 100PHR;
[0008] Reinforcing agent 10-30PHR;
[0009] Filler 80-120PHR;
[0010] Plasticizer 5-60PHR;
[0011] Deodorant 2-30PHR;
[0012] Anti-aging agent 0.5-10PHR;
[0013] Curing agent 1.5-10PHR;
[0014] Auxiliary cross-linking agent 0.5-6PHR.
[0015] Preferably, the raw rubber is styrene-butadiene rubber (SBR) or ethylene-propylene rubber (EPDM).
[0016] Preferably, the reinforcing agent is at least one of white carbon black and carbon black.
[0017] Preferably, the filler is organically modified montmorillonite.
[0018] Preferably, the preparation process of the organic modified montmorillonite comprises the following steps: preparing the required montmorillonite and quaternary ammonium salt (including hexadecyltrimethylammonium bromide or CTAB);
[0019] Mixing montmorillonite with deionized water to prepare a montmorillonite aqueous solution;
[0020] Dissolving the quaternary ammonium salt in an appropriate amount of water to prepare an intercalation agent aqueous solution;
[0021] In a water bath at 60-90° C., uniformly mixing the montmorillonite aqueous solution and the intercalation agent aqueous solution to form an organic modified montmorillonite aqueous solution;
[0022] The mixed solution is cooled and filtered, washed to remove unreacted quaternary ammonium salt, and then dried at 50-60°C for 1-3 hours; the drying reaction is continued at 120°C for 1-2 hours to ensure complete drying; after cooling, the organic modified montmorillonite is obtained.
[0023] Preferably, the plasticizer is pharmacopoeia grade white hydrogenated paraffin oil.
[0024] Preferably, the deodorant is an adsorptive deodorant; it absorbs small molecules with odors that remain or are generated during the processing of rubber, thereby achieving a low-odor effect.
[0025] Preferably, the antioxidant is at least one of 4,4'-di(phenylisopropyl)diphenylamine, 2-mercaptobenzimidazole zinc salt, 1,3-dihydro-4-methyl-2-mercaptobenzimidazole zinc, and 2-methylmercaptobenzimidazole.
[0026] Preferably, the vulcanizing agent is at least one of di-tert-butyl peroxide isopropylbenzene and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and the ratio of the vulcanizing agent to the raw rubber is in the range of 1.5% to 10%.
[0027] Preferably, the auxiliary cross-linking agent is at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, and 1,3,5-triallyl cyanurate.
[0028] Based on the above improved formula components of the novel rubber compound, the present invention also provides a method for preparing the novel rubber compound, comprising the following steps:
[0029] 1) Material preparation: weigh raw rubber, reinforcing agent and antioxidant according to the formula to form ingredient A;
[0030] preparing organic modified montmorillonite as a filler to form ingredient B;
[0031] Weighing a deodorant to form ingredient C;
[0032] Weighing a vulcanizing agent and a co-crosslinking agent to form a batch D;
[0033] 2) The first mixing:
[0034] Put ingredient A into internal mixer, mix for 60 to 120 seconds, then lift the hammer and clean it;
[0035] Add ingredient B and continue mixing for 60 to 120 seconds to ensure that the filler is evenly dispersed;
[0036] When the temperature of the rubber compound reaches 135-150℃, add ingredient C, mix for 10-60 seconds, then lift the hammer and clean;
[0037] Mix for 10 to 240 seconds, control the temperature at 145 to 165°C, unload and make a preliminary mixed rubber, and leave it for more than 16 hours;
[0038] 3) Second mixing: put the preliminary mixed rubber and ingredient D into the internal mixer, mix for 20 to 50 seconds and then lift the hammer to clean;
[0039] Continue mixing for 20 to 30 seconds, controlling the temperature of the rubber compound at 85-115°C;
[0040] After unloading and parking for more than 16 hours, the final rubber mix is prepared.
[0041] Beneficial effects: 1. Selecting organic quaternary ammonium salt modified montmorillonite as a filler and a suitable reinforcing agent can improve the tensile strength, elongation at break and compression resistance of rubber compound. At the same time, selecting pharmacopoeia grade white hydrogenated paraffin oil as a plasticizer, combined with the high-efficiency adsorption capacity of organic modified montmorillonite, can adsorb and fix low molecular weight volatile substances in the rubber compound system, reducing odor and VOC emissions.
[0042] 2. By using specific vulcanizing agents and co-crosslinking agents, the vulcanization speed is increased while maintaining high heat resistance.
[0043] 3. Use peroxide vulcanization system and specific antioxidants to improve the heat resistance of the material. DETAILED DESCRIPTION
[0044] The present invention is described in detail below with reference to the embodiments, but is not intended to limit the present invention.
[0045] A novel rubber compound comprises the following components in parts by weight (PHR):
[0046] Raw rubber 100PHR;
[0047] Reinforcing agent 10-30PHR;
[0048] Filler 80-120PHR;
[0049] Plasticizer 5-60PHR;
[0050] Deodorant 2-30PHR;
[0051] Anti-aging agent 0.5-10PHR;
[0052] Curing agent 1.5-10PHR;
[0053] Auxiliary cross-linking agent 0.5-6PHR.
[0054] As a further improvement of the embodiment of the present invention, the raw rubber is styrene-butadiene rubber (SBR) or ethylene-propylene rubber (EPDM),
[0055] As a further improvement of the embodiment of the present invention, the reinforcing agent is at least one of white carbon black and carbon black.
[0056] As a further improvement of the embodiment of the present invention, the filler is organic modified montmorillonite.
[0057] As a further improvement of the embodiment of the present invention, the preparation process of the organic modified montmorillonite comprises the following steps: preparing the required montmorillonite and quaternary ammonium salt (including hexadecyltrimethylammonium bromide or CTAB);
[0058] Mixing montmorillonite with deionized water to prepare a montmorillonite aqueous solution;
[0059] Dissolving the quaternary ammonium salt in an appropriate amount of water to prepare an intercalation agent aqueous solution;
[0060] In a water bath at 60-90° C., uniformly mixing the montmorillonite aqueous solution and the intercalation agent aqueous solution to form an organic modified montmorillonite aqueous solution;
[0061] The mixed solution is cooled and filtered, washed to remove unreacted quaternary ammonium salt, and then dried at 50-60°C for 1-3 hours; the drying reaction is continued at 120°C for 1-2 hours to ensure complete drying; after cooling, the organic modified montmorillonite is obtained.
[0062] Organic quaternary ammonium salts are the most commonly used cationic surfactants in MMT organic modification. Since organic quaternary ammonium salts are large in size, after entering the interlayer of MMT, the montmorillonite changes from hydrophilic to lipophilic, thereby improving the compatibility with the rubber matrix; it can also effectively increase the interlayer spacing, which is beneficial to the intercalation of polymer chains and also improves thermal stability.
[0063] Adding organic modified montmorillonite to EPDM rubber as a filler can not only improve the mechanical properties of the material, but also effectively adsorb and fix low molecular weight volatile substances in the rubber mixing system.
[0064] As a further improvement of the embodiment of the present invention, the plasticizer is pharmacopoeia grade white hydrogenated paraffin oil. The flash point of the plasticizer is above 260°C; the aromatic content of the plasticizer is below 0.1%. The viscosity of the plasticizer (100°C) is above 10 mm / s. The ratio of the plasticizer to the raw rubber is between 5% and 60%. In this way, the processing performance of the mixed rubber can be guaranteed, and the generation of volatile small molecules can be reduced, achieving a low odor effect.
[0065] As a further improvement of the embodiment of the present invention, the deodorant is an adsorptive deodorant; it absorbs small molecules with odors that remain or are generated during the processing of rubber, thereby achieving a low-odor effect.
[0066] As a further improvement of the embodiment of the present invention, the antioxidant is at least one of 4,4'-di(phenylisopropyl)diphenylamine, 2-mercaptobenzimidazole zinc salt, 1,3-dihydro-4-methyl-2-mercaptobenzimidazole zinc, and 2-methylmercaptobenzimidazole.
[0067] As a further improvement of the embodiment of the present invention, the vulcanizing agent is at least one of di-tert-butyl peroxide isopropylbenzene and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; the ratio of the vulcanizing agent to the raw rubber is between 1.5% and 10%; the use of a peroxide vulcanization system can improve the high heat resistance of the material, and the number of component types is relatively small, and the decomposition product has a low odor level after volatilization and adsorption. The use of a peroxide system in combination with hydrogenated white paraffin oil can reduce the amount of peroxide used and the amount of decomposition products, which is beneficial to reducing the odor of rubber.
[0068] As a further improvement of the embodiment of the present invention, the auxiliary cross-linking agent is at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, and 1,3,5-triallyl cyanurate.
[0069] In the specific implementation process, the components of the new rubber compound involved in Examples 1-4 and Comparative Examples 1-2 are composed by weight as shown in Table 1:
[0070]
[0071]
[0072] Based on the above improved formula components of the novel rubber compound, the present invention also provides a method for preparing the novel rubber compound, comprising the following steps:
[0073] 1) Material preparation: weigh raw rubber, reinforcing agent and antioxidant according to the formula to form ingredient A;
[0074] preparing organic modified montmorillonite as a filler to form ingredient B;
[0075] Weighing a deodorant to form ingredient C;
[0076] Weighing a vulcanizing agent and a co-crosslinking agent to form a batch D;
[0077] 2) The first mixing:
[0078] Put ingredient A into internal mixer, mix for 60 to 120 seconds, then lift the hammer and clean it;
[0079] Add ingredient B and continue mixing for 60 to 120 seconds to ensure that the filler is evenly dispersed;
[0080] When the temperature of the rubber compound reaches 135-150℃, add ingredient C, mix for 10-60 seconds, then lift the hammer and clean;
[0081] Mix for 10 to 240 seconds, control the temperature at 145 to 165°C, unload and make a preliminary mixed rubber, and leave it for more than 16 hours;
[0082] 3) Second mixing: put the preliminary mixed rubber and ingredient D into the internal mixer, mix for 20 to 50 seconds and then lift the hammer to clean;
[0083] Continue mixing for 20 to 30 seconds, controlling the temperature of the rubber compound at 85-115°C;
[0084] After unloading and parking for more than 16 hours, the final rubber mix is prepared.
[0085] The specific process parameters of the preparation method of the new rubber compound involved in Examples 1-4 and Comparative Examples 1-2 are shown in Table 2 below:
[0086]
[0087] Test plan
[0088] According to the schemes of Examples 1-4 and Comparative Examples 1-2 shown in Table 1 above, the schemes for testing and evaluating the physical properties of the rubber honey compound products are as follows:
[0089] Hardness test: Use a Shore durometer to perform a hardness test in accordance with GB / T 531 standard to determine the hardness grade of the rubber.
[0090] Tensile properties and elongation at break test: According to GB / T 528 standard, a universal material testing machine is used to test the tensile strength and elongation at break to evaluate the strength and elongation of rubber.
[0091] Hot air aging test: According to GB / T3512 standard, the rubber samples were subjected to a hot air aging test at 150°C for 168 hours to evaluate their heat aging resistance.
[0092] Compression set test: According to GB / T 7759 standard, the rubber sample was subjected to compression test at 150°C for 72 hours to determine its compression set rate.
[0093] Odor rating: According to VDA 270, rubber samples are rated for odor to determine their odor intensity.
[0094] The physical property test results of the rubber products of Comparative Examples 1-2 and Examples 1-4 are shown in Table 3 below:
[0095]
[0096] As can be seen from Table 3, the rubber compound of Examples 1-4 of the present invention has good physical and mechanical properties, and its aging resistance is significantly better than that of Comparative Examples 1-2, and its compression permanent deformation performance is significantly lower than that of Comparative Examples 1-2, indicating that the new rubber compound has a stronger ability to maintain its shape at high temperatures. At the same time, the odor level of Examples 1-4 is significantly lower than that of Comparative Examples 1-2, indicating that its odor is more in line with environmental protection and use requirements.
[0097] In addition, the rubber compound of Example 3 exhibits good comprehensive performance in terms of aging resistance, compression set performance, odor level and physical and mechanical properties. These characteristics make it an excellent choice, especially in applications requiring high-performance rubber materials.
[0098] The above embodiments are provided for persons familiar with the art to implement or use the present invention. Personnel familiar with the art can make various modifications or changes to the above embodiments without departing from the inventive concept of the present invention. Therefore, the protection scope of the present invention is not limited to the above embodiments, but should be the maximum scope of the innovative features mentioned in the claims.
Claims
1. A novel rubber compound, characterized in that: The composition comprises the following parts by weight (PHR): Raw rubber 100PHR; Reinforcing agent 10-30PHR; Filler 80-120PHR; Plasticizer 5-60PHR; Deodorant 2-30PHR; Anti-aging agent 0.5-10PHR; Curing agent 1.5-10PHR; Cross-linking agent 0.5-6PHR; The raw rubber is ethylene-propylene rubber (EPDM); The reinforcing agent is at least one of white carbon black and carbon black; The filler is organic modified montmorillonite.
2. A novel rubber compound according to claim 1, characterized in that: The plasticizer is pharmacopoeia grade white hydrogenated paraffin oil.
3. A novel rubber compound according to claim 1, characterized in that: The deodorant is an adsorptive deodorant.
4. A novel rubber compound according to claim 1, characterized in that: The antioxidant is at least one of 4,4'-di(phenylisopropyl)diphenylamine, 2-mercaptobenzimidazole zinc salt, 1,3-dihydro-4-methyl-2-mercaptobenzimidazole zinc, and 2-methylmercaptobenzimidazole.
5. A novel rubber compound according to claim 1, characterized in that: The vulcanizing agent is at least one of di-tert-butyl peroxide isopropylbenzene and 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane; the ratio of the vulcanizing agent to the raw rubber is in the range of 1.5% to 10%.
6. A novel rubber compound according to claim 1, characterized in that: The auxiliary cross-linking agent is at least one of triallyl isocyanurate, trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, and 1,3,5-triallyl cyanurate.
7. The method for preparing the novel rubber compound according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: 1) Material preparation: weigh raw rubber, reinforcing agent and antioxidant according to the formula to form ingredient A; preparing organic modified montmorillonite as a filler to form ingredient B; Weighing a deodorant to form ingredient C; Weighing a vulcanizing agent and a co-crosslinking agent to form a batch D; 2) The first mixing: Put ingredient A into internal mixer, mix for 60 to 120 seconds, then lift the hammer and clean it; Add ingredient B and continue mixing for 60 to 120 seconds to ensure that the filler is evenly dispersed; When the temperature of the rubber compound reaches 135-150℃, add ingredient C, mix for 10-60 seconds, then lift the hammer and clean; Mix for 10 to 240 seconds, control the temperature at 145 to 165°C, unload and make a preliminary mixed rubber, and leave it for more than 16 hours; 3) Second mixing: put the preliminary mixed rubber and ingredient D into the internal mixer, mix for 20 to 50 seconds and then lift the hammer to clean; Continue mixing for 20 to 30 seconds, controlling the temperature of the rubber compound at 85-115°C; After unloading and parking for more than 16 hours, the final rubber mix is prepared.
Citation Information
Cited By
Rubber formaldehyde removal additive and preparation method thereof
CN122302378A