Highly-modified polystyrene blending foaming material as well as preparation method and application thereof

Synthesizing high-modified polystyrene blended foaming materials through one-step extrusion process, solving the problems of high cost of foaming materials and high waste, achieving performance improvement and environmentally friendly production, and is suitable for high-end packaging fields, especially in liquid crystals, Mobile phone tablet and silicon chip packaging.

CN119081305AInactive Publication Date: 2024-12-06GANSU QIANYI NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411417513.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing foaming materials are costly, and a large amount of waste is generated during the production process, and their performance is not enough to meet the needs of the high-end packaging field.

Method used

Polystyrene, nucleating agent, pentane and citric acid are used to synthesize high-modified polystyrene blended foamed materials through a one-step extrusion process to reduce waste emissions and improve material performance.

Benefits of technology

It realizes low-cost and environmentally friendly foaming material preparation, and its performance is close to imported EPO. It is suitable for high-end packaging fields, especially in liquid crystal, mobile phone tablets and silicon chip packaging, shortening molding time and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of foam materials and preparation thereof, and relates to a highly modified polystyrene blended foam material and a preparation method and application thereof, the highly modified polystyrene blended foam material comprises the following raw materials by mass: 91%-94% of polystyrene, 1%-2% of a nucleating agent, 2%-5.5% of pentane and 1%-3% of citric acid; the nucleating agent is calcium carbonate or calcium oxide. The high-modified polystyrene blending foaming material is synthesized from polystyrene, the nucleating agent, pentane and citric acid by adopting an extrusion one-step process, the cost is low, the emission of three wastes is reduced, the material performance is good, and the high-modified polystyrene blending foaming material can be well applied to the field of high-end packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming materials and preparation thereof, and relates to a highly modified polystyrene blended foaming material and a preparation method and application thereof. Background Art

[0002] Foaming agent refers to a substance that can be vaporized to produce bubbles inside a substance to make it a porous substance, such as foam plastics, foam rubber, foam resin and other foaming materials. Since the foamed materials have the characteristics of heat preservation, heat insulation, and waterproof, they are widely used in the fields of construction, home appliances, packaging, transportation, etc.

[0003] Commonly used materials in the packaging field include EPS (expanded polystyrene) and non-crosslinked closed-cell EPE (polyethylene foam), but EPS has the disadvantages of not being able to withstand multiple impacts, being brittle, easy to break, and having low tensile strength; EPE has the disadvantages of being difficult to form into films and being expensive. Therefore, researchers have proposed EPO foams made by foaming polyolefin and vinyl aromatic monomer interpolymer resin particles, wherein the interpolymer resin particles are composed of uncrosslinked polyolefin (polyethylene, polypropylene) and vinyl aromatic monomer (styrene), and the vinyl aromatic monomer is polymerized by a suspension process to form an interpenetrating network of polyolefin and polymerized vinyl aromatic monomer particles. However, EPO is mostly imported products, such as the EPO produced by Nufa Company, named Arcel, which is composed of 30% polyethylene and 70% polystyrene; then air bubbles are formed inside it by chemical methods to form a lightweight sound insulation, heat insulation, and energy absorption material; but due to the high price of EPO synthesis, the cost is relatively high. In addition, the traditional process of foaming materials is to use chemical methods, but its disadvantage is that a large amount of three wastes will be generated, which does not meet the requirements of green environmental protection.

[0004] In summary, how to provide a new foaming material with low cost, less three wastes and better performance is a technical problem that needs to be solved at present. Summary of the invention

[0005] In view of the technical problems of high cost, many three wastes and poor performance of foaming materials in the background technology, the present invention provides a highly modified polystyrene blended foaming material and a preparation method and application thereof.

[0006] The invention adopts polystyrene, a nucleating agent, pentane and citric acid, and adopts an extrusion one-step process to synthesize a high-modified polystyrene blended foaming material, which has low cost, reduces the emission of three wastes, and has good material properties, and can be well used in the field of high-end packaging.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A highly modified polystyrene blended foaming material comprises the following raw materials in different mass fractions:

[0009] 91% to 94% polystyrene, 1% to 2% nucleating agent, 2% to 5.5% pentane and 1% to 3% citric acid; the nucleating agent is calcium carbonate or calcium oxide.

[0010] It is further defined that the mass fraction of the pentane is 5% to 5.5%; the mass fraction of the pentane is 5% to 5.5%; and the mass fraction of the polystyrene is 91% to 93%.

[0011] It is further defined that the high-modified polystyrene blended foam material has an average particle size of 0.8 mm to 1.5 mm, a foam filling thickness of 5 mm to 8 mm, and a foaming density of 0.15 kg / cm 3 ~0.50kg / cm 3 .

[0012] The preparation method of the highly modified polystyrene blended foaming material comprises the following steps:

[0013] S1. Prepare each raw material according to the mass fraction;

[0014] S2, mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture;

[0015] S3, continuously adding the mixed material into a twin-screw extruder, and simultaneously adding pentane and citric acid into the twin-screw extruder, and melting the mixed material, pentane and citric acid at a temperature of 130° C. to 200° C., mixing and plasticizing, and the formed material is extruded, and is instantly cooled and pelletized;

[0016] S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material.

[0017] It is further defined that in step S3, the feeding speed of the twin-screw extruder is 15r / min-25r / min, the main engine speed is 150r / min-260r / min, the melt mixer speed is 10r / min-25r / min, the die head temperature is 240°C-300°C, and the water tank temperature is controlled at 40°C-50°C.

[0018] It is further defined that in step S3, instantaneous cooling is achieved by cooling water at a temperature of 0.48 MPa to 0.65 MPa.

[0019] It is further defined that in step S4, the mass of the coating agent added is 1‰-2‰ of the total mass of the material after pelletizing.

[0020] It is further defined that the coating agent is zinc stearate or tristearic acid.

[0021] The application of the highly modified polystyrene blended foaming material in electronic product packaging.

[0022] The highly modified polystyrene blended foaming material is used in the packaging of liquid crystals, mobile phones, tablets or silicon chips.

[0023] The beneficial effects of the present invention are:

[0024] 1. The main components of the foaming material of the present invention are polystyrene, a nucleating agent, pentane and citric acid. It is manufactured by a one-step extrusion process, has low cost, and can be well used in the field of high-end packaging, such as packaging of electronic products such as liquid crystals (panels, glass, televisions), mobile phone tablets, and silicon chips.

[0025] 2. Compared with the traditional EPO process, the high-modified polystyrene blended foam material adopts physical principles for mixing, extrusion and granulation, which is more environmentally friendly and energy-saving. It reduces the emission of three wastes compared with the traditional process (chemical reaction), and complies with the national policy of safe and environmentally friendly production. It is also included in the 6th category of international foam waste recycling, reducing the odor of the product and improving the stability and corrosion resistance of the product.

[0026] 3. The high-modified polystyrene foam material prepared by the present invention is close to EPO in terms of material properties and use functions and fields, and has higher physical strength than imported EPO materials. However, it adopts low-pressure and low-temperature foaming, the temperature does not exceed 88°C, and the aging time is within 4 to 6 hours. The molding time is relatively short, while the aging time of imported EPO is 2-3 days. The production efficiency is improved. Under normal circumstances, the foaming loss of high-modified polystyrene is only 4% to 5%, which can meet the use of more occasions. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] The invention provides a highly modified polystyrene blended foaming material, comprising the following raw materials in mass fractions: 91% to 94% polystyrene, 1% to 2% nucleating agent, 2% to 5.5% pentane and 1% to 3% citric acid; the nucleating agent is calcium carbonate or calcium oxide.

[0029] Preferably, the mass fraction of polystyrene is 91%, 92%, 93% or 94%; the mass fraction of nucleating agent is 1%, 1.5% or 2%; the mass fraction of pentane is 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or 5.5%; the mass fraction of citric acid is 1%, 1.5%, 2%, 2.5% or 3%.

[0030] Preferably, the mass fraction of pentane is 5% to 5.5%.

[0031] The high-modified polystyrene foam material provided by the present invention has an average particle size of 0.8 mm to 1.5 mm, a foam filling thickness of 5 mm to 8 mm, and a foaming density of 0.15 kg / cm 3 ~0.50kg / cm 3 .

[0032] The present invention also provides a method for preparing a highly modified polystyrene blended foam material, comprising the following steps:

[0033] S1. Prepare each raw material according to the mass fraction;

[0034] S2, mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture;

[0035] S3, continuously adding the mixed material into a twin-screw extruder, and simultaneously adding pentane and citric acid into the twin-screw extruder, and melting the mixed material, pentane and citric acid at a temperature of 130° C. to 200° C., mixing and plasticizing, and the formed material is extruded, and is instantly cooled and pelletized;

[0036] In step S3 of the present invention, the feeding speed of the twin-screw extruder is 15r / min-25r / min, the main engine speed is 150r / min-260r / min, the melt mixer speed is 10r / min-25r / min, the die head temperature is 240°C-300°C, and the water tank temperature is controlled at 40°C-50°C.

[0037] In step S3 of the present invention, instant cooling is achieved by cooling water at 0.48Mpa to 0.65Mpa.

[0038] S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material.

[0039] In step S4 of the present invention, the mass of the coating agent added is 1‰-2‰ of the total mass of the material after pelletizing.

[0040] Preferably, the coating agent is zinc stearate or tristearic acid.

[0041] The highly modified polystyrene blended foam material prepared by the present invention adopts a one-step extrusion method, has less three wastes, is environmentally friendly, and has readily available raw materials. It has extremely strong performance and can be well used in high-end electronic product packaging, especially in liquid crystal, mobile phone tablet or silicon chip packaging.

[0042] The highly modified polystyrene blended foam material and the preparation method thereof provided by the present invention are described in detail below in conjunction with several groups of embodiments.

[0043] It should be noted that, unless otherwise specified, the chemical raw materials used in the following examples are all conventional commercial products in the art.

[0044] Example 1

[0045] This embodiment provides a highly modified polystyrene blended foaming material, comprising the following raw materials in the following mass fractions: 91% polystyrene, 2% nucleating agent, 4% pentane and 3% citric acid; the nucleating agent is calcium carbonate.

[0046] The preparation method of the highly modified polystyrene blended foam material provided in this embodiment comprises the following steps:

[0047] S1. Prepare each raw material according to the mass fraction; the total mass of the high-modified polystyrene blended foam material is 100 parts, and the mass ratio of polystyrene, nucleating agent, pentane and citric acid is 91:2:4:3.

[0048] S2. Mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture.

[0049] S3. The mixed material is continuously added into a twin-screw extruder, and pentane and citric acid are added into the twin-screw extruder at the same time. The mixed material, pentane and citric acid are melted and mixed and plasticized at a temperature of 130° C. The formed material is extruded, and is instantly cooled and pelletized.

[0050] Preferably, in step S3, the feeding speed of the twin-screw extruder is 15 r / min, the main engine speed is 260 r / min, the melt mixer speed is 25 r / min, the die temperature is 300° C., and the water tank temperature is controlled at 50° C. Instant cooling is completed by cooling water at 0.48 Mpa.

[0051] S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material. The added mass of the coating agent is 2‰ of the total mass of the pelletized material. The coating agent is zinc stearate.

[0052] Example 2

[0053] This embodiment provides a highly modified polystyrene blended foaming material, comprising the following raw materials in different mass fractions: 92% polystyrene, 1.5% nucleating agent, 5.5% pentane and 1% citric acid; the nucleating agent is calcium carbonate.

[0054] The preparation method of the highly modified polystyrene blended foam material provided in this embodiment comprises the following steps:

[0055] S1. Prepare each raw material according to the mass fraction; the total mass of the high-modified polystyrene blended foaming material is 100 parts, and the mass ratio of polystyrene, nucleating agent, pentane and citric acid is 92:1.5:5.5:1.

[0056] S2. Mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture.

[0057] S3. The mixed material is continuously added into a twin-screw extruder, and pentane and citric acid are added into the twin-screw extruder at the same time. The mixed material, pentane and citric acid are melted and mixed and plasticized at a temperature of 150° C. The formed material is extruded, and is instantly cooled and pelletized.

[0058] Preferably, in step S3, the feeding speed of the twin-screw extruder is 25 r / min, the main engine speed is 150 r / min, the melt mixer speed is 10 r / min, the die temperature is 240° C., and the water tank temperature is controlled at 40° C. Instant cooling is completed by cooling water at 0.65 MPa.

[0059] S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material. The added mass of the coating agent is 1‰ of the total mass of the pelletized material. The coating agent is zinc stearate.

[0060] Example 3

[0061] This embodiment provides a highly modified polystyrene blended foaming material, comprising the following raw materials in different mass fractions: 92% polystyrene, 1.5% nucleating agent, 5% pentane and 1.5% citric acid; the nucleating agent is calcium carbonate.

[0062] The preparation method of the highly modified polystyrene blended foam material provided in this embodiment comprises the following steps:

[0063] S1. Prepare each raw material according to the mass fraction; the total mass of the high-modified polystyrene blended foaming material is 100 parts, and the mass ratio of polystyrene, nucleating agent, pentane and citric acid is 92:1.5:5:1.5.

[0064] S2. Mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture.

[0065] S3. The mixed material is continuously added into a twin-screw extruder, and pentane and citric acid are added into the twin-screw extruder at the same time. The mixed material, pentane and citric acid are melted and mixed and plasticized at a temperature of 160° C. The formed material is extruded, and is instantly cooled and pelletized.

[0066] Preferably, in step S3, the feeding speed of the twin-screw extruder is 20 r / min, the main engine speed is 200 r / min, the melt mixer speed is 15 r / min, the die temperature is 260° C., and the water tank temperature is controlled at 45° C. Instant cooling is completed by cooling water at 0.55 MPa.

[0067] S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material. The added mass of the coating agent is 1‰ of the total mass of the pelletized material. The coating agent is zinc stearate.

[0068] Example 4

[0069] This embodiment provides a highly modified polystyrene blended foaming material, comprising the following raw materials in different mass fractions: 94% polystyrene, 1% nucleating agent, 2% pentane and 3% citric acid; the nucleating agent is calcium carbonate.

[0070] The preparation method of the highly modified polystyrene blended foam material provided in this embodiment comprises the following steps:

[0071] S1. Prepare each raw material according to the mass fraction; the total mass of the high-modified polystyrene blended foaming material is 100 parts, and the mass ratio of polystyrene, nucleating agent, pentane and citric acid is 94:1:2:3.

[0072] S2. Mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture.

[0073] S3. The mixed material is continuously added into a twin-screw extruder, and pentane and citric acid are added into the twin-screw extruder at the same time. The mixed material, pentane and citric acid are melted and mixed and plasticized at a temperature of 200° C. The formed material is extruded, and is instantly cooled and pelletized.

[0074] Preferably, in step S3, the feeding speed of the twin-screw extruder is 25 r / min, the main engine speed is 240 r / min, the melt mixer speed is 20 r / min, the die temperature is 280° C., and the water tank temperature is controlled at 45° C. Instant cooling is completed by cooling water at 0.6 Mpa.

[0075] S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material. The added mass of the coating agent is 1‰ of the total mass of the pelletized material. The coating agent is zinc stearate.

[0076] The above embodiments are several groups of preferred implementations of the present invention, wherein the nucleating agent can be replaced by calcium oxide, and the coating agent can be replaced by tristearic acid.

[0077] The physical properties of the high-modified polystyrene foam material prepared above were tested, and the average particle size was 0.8 mm to 1.5 mm, the foam filling thickness was 5 mm to 8 mm, and the foaming density was 0.15 kg / cm 3 ~0.50kg / cm 3. At the same time, the high-modified polystyrene blended foaming material formed in the above embodiment has good performance. When low-pressure and low-temperature foaming is adopted, the temperature does not exceed 88°C, and the aging time is within 4 to 6 hours. The molding time is relatively short. Compared with the aging time of imported EPO of 2-3 days, the production efficiency is improved. Under normal circumstances, the foaming loss of high-modified polystyrene is only 4% to 5%. Therefore, the high-modified polystyrene blended foaming material prepared by the present invention can be well used in the field of high-end packaging, especially in the packaging of electronic products such as liquid crystal (panel, glass, TV), mobile phone tablet, silicon chip, etc., to reduce costs, shorten molding time, and improve molding efficiency.

[0078] Furthermore, the performance of the foamed material prepared by the present invention is verified through experiments.

[0079] The purpose of the test is to select the highly modified polystyrene blended foaming material provided in Example 2 and compare its performance with the EPO foaming material imported by Nufa Company.

[0080] The test process is: when the foaming ratio is 20 times, 25 times, 30 times and 40 times, the density, compression strength, tensile strength at break, puncture strength and flexural stress performance indicators of the above two foaming materials are measured respectively.

[0081] The test methods for performance indicators are based on the standards: density uses GB / T6343-2009, compression strength uses GB / T8813-2008, tensile strength at break uses ASTM-D63814, puncture strength uses ASTM-F13016, and flexural stress uses ASTM-C203.

[0082] The performance test results are shown in Table 1.

[0083] Table 1 Comparison of performance of two foaming materials

[0084]

[0085] As can be seen from Table 1, by comparing the high-modified polystyrene blended foaming material prepared by the present invention with the imported EPO, the high-modified polystyrene blended foaming material is close to EPO in terms of material properties, usage functions and fields. However, the cost of the high-modified polystyrene blended foaming material provided by the present invention is much lower than the preparation cost of imported EPO in terms of raw materials and preparation method, and it produces less three wastes and is more environmentally friendly.

[0086] It can be seen that the high-modified polystyrene blended foam material prepared by the present invention has achieved localized production and manufacturing, and the cost is lower than the current market price of imported EPO. It can be used as a new material to replace imported EPO in high-end packaging materials, especially in the packaging of liquid crystals, mobile phone tablets or silicon chips.

[0087] Obviously, the above embodiments are merely examples for clearly illustrating the technical solutions of the present invention, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above descriptions, and it is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the present invention.

Claims

1. A highly modified polystyrene blended foaming material, It is characterized in that Including the following mass fractions of each raw material: 91% to 94% polystyrene, 1% to 2% nucleating agent, 2% to 5.5% pentane and 1% to 3% citric acid; the nucleating agent is calcium carbonate or calcium oxide.

2. The highly modified polystyrene blended foaming material according to claim 1, It is characterized in that The mass fraction of the pentane is 5% to 5.5%; the mass fraction of the polystyrene is 91% to 93%.

3. The highly modified polystyrene blended foaming material according to claim 1, It is characterized in that The high-modified polystyrene blended foaming material has an average particle size of 0.8 mm to 1.5 mm, a foam filling thickness of 5 mm to 8 mm, and a foaming density of 0.15 kg / cm 3 ~0.50kg / cm 3 .

4. The method for preparing the highly modified polystyrene blended foaming material according to claim 1, It is characterized in that The preparation method comprises the following steps: S1. Prepare each raw material according to the mass fraction; S2, mixing polystyrene and a nucleating agent in a closed environment to obtain a mixture; S3, continuously adding the mixed material into a twin-screw extruder, and simultaneously adding pentane and citric acid into the twin-screw extruder, and melting the mixed material, pentane and citric acid at a temperature of 130° C. to 200° C., mixing and plasticizing, and the formed material is extruded, and is instantly cooled and pelletized; S4, mixing the coating agent with the pelletized material to obtain a high-modified polystyrene foam material.

5. The preparation method according to claim 4, It is characterized in that In step S3, the feeding speed of the twin-screw extruder is 15r / min-25r / min, the main engine speed is 150r / min-260r / min, the melt mixer speed is 10r / min-25r / min, the die temperature is 240°C-300°C, and the water tank temperature is controlled at 40°C-50°C.

6. The preparation method according to claim 4, It is characterized in that In the step S3, instant cooling is performed by cooling water at a temperature of 0.48 MPa to 0.65 MPa.

7. The preparation method according to claim 4, It is characterized in that In step S4, the mass of the coating agent added is 1‰-2‰ of the total mass of the material after pelletizing.

8. The preparation method according to claim 7, It is characterized in that The coating agent is zinc stearate or tristearic acid.

9. Use of the highly modified polystyrene blended foam material as claimed in claim 1 in electronic product packaging.

10. Use of the highly modified polystyrene blended foam material according to claim 1 in packaging of liquid crystal, mobile phone tablet or silicon chip.