Photosensitive emulsion for screen printing plate and preparation method thereof
By adding ingredients such as leveling agent, blue tint and adhesion promoter to the photosensitive emulsion of the printed screen, combined with emulsion polymerization, the problem of insufficient adhesion of the UV emulsion is solved, and the adhesion of the printed screen is significantly improved. The service life of the screen avoids cracking and explosive versions.
Patent Information
- Application Number
- CN202411206862.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing UV emulsions are insufficient in the use of screen printing screens, which leads to cracking and bursting of the printed screens with the increase in the number of printings, affecting the service life of the screens.
A photosensitive emulsion for printing screens was developed to synthesize polyvinyl acetate emulsions by emulsion polymerization, and add leveling agents, blue chromatic paste, adhesion promoter and vapor phase silica to improve the photosensitive emulsion. Adhesion, mixing and stirring using specific proportions of ingredients and process steps to form a photosensitive emulsion with high adhesion.
It significantly improves the adhesion of the photosensitive emulsion on the printed screen steel mesh, extends the service life of the printed screen, and avoids cracking and explosive versions of the screen.
Smart Images

Figure BDA0005019266140000011 
Figure BDA0005019266140000031 
Figure FDA0005019266130000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of emulsions, and in particular, relates to a photosensitive emulsion for printing screens and a preparation method thereof. Background Art
[0002] Screen printing is a process used in mass production of solar cells. Its purpose is to print a conductive paste containing metal on a silicon wafer through the mesh of the screen to form a circuit and / or electrode. At present, the screen printing screen for solar cell electrodes generally uses a metal steel mesh as the material of the printing area, and its periphery is composited with a polyester mesh to give the screen a certain resilience to achieve the purpose of printing. Conventional plate making uses UV emulsion to fill and repair the overlapping area of the periphery of the steel mesh and the composite of the polyester mesh. However, due to the insufficient adhesion of the UV emulsion, as the number of printings increases, the printed screen is prone to cracking and explosion, which affects the service life of the screen. Summary of the invention
[0003] The purpose of the embodiment of the present invention is to provide a photosensitive emulsion for a printing screen that can prevent the printing screen from cracking and bursting and thus increase the service life of the screen.
[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide a photosensitive emulsion for printing screen, comprising the following components in parts by weight:
[0005]
[0006]
[0007] Optionally, based on the weight of each raw material component, the polyvinyl acetate emulsion includes 4 to 6 parts of polyvinyl alcohol, 50 to 60 parts of deionized water, 0.5 to 1 part of a surfactant, 303 to 406 parts of monomer vinyl acetate, 0.53 to 1.06 parts of an initiator, 1.1 to 2.2 parts of a buffer, 3 to 5 parts of acrylic acid, 50 to 70 parts of ethyl acrylate and 1 to 2 parts of dipropylene phthalate.
[0008] Optionally, the surfactant is Lutensol TO-7.
[0009] Optionally, the initiator is potassium persulfate.
[0010] Optionally, the buffer is sodium acetate.
[0011] Optionally, the concentration of the polyvinyl alcohol aqueous solution is 15% to 20%.
[0012] Optionally, the adhesion promoter is Easepi 516.
[0013] Optionally, the fumed silica is fumed silica R 972, a viscosity-enhancing filler.
[0014] Optionally, based on the weight of each raw material component, the photosensitive emulsion for printing screen further includes 0.5 to 1 part of green diazo photosensitizer solution.
[0015] Another object of the embodiment of the present invention is to provide a method for preparing a photosensitive emulsion for a printing screen that can prevent the printing screen from cracking and bursting and thus increase the service life of the screen.
[0016] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a photosensitive emulsion for printing screen, comprising the following steps:
[0017] Step S01: weighing the raw materials of the photosensitive emulsion for printing screen according to any of the above embodiments or schemes;
[0018] Step S02: stirring and mixing the polyvinyl acetate emulsion and the polyvinyl alcohol aqueous solution to obtain a mixed solution A;
[0019] Step S03: adding a leveling agent, a blue color paste, an adhesion promoter and fumed silica to the mixed solution A, stirring and mixing, to obtain a mixture B;
[0020] Step S04: stirring the mixture B in a disperser for 30 to 60 minutes to obtain a mixture C;
[0021] Step S05: Filter the mixture C, add a green diazo photosensitizer solution, stir evenly, and let stand to defoam, to obtain a photosensitive emulsion.
[0022] Compared with the prior art, the one or more technical solutions in the embodiments of the present invention have at least one of the following beneficial effects:
[0023] The photosensitive emulsion for printing screen in the embodiment of the present invention and the preparation method thereof include, by weight, 200-260 parts of polyvinyl acetate emulsion, 50-100 parts of polyvinyl alcohol aqueous solution, 1-2 parts of leveling agent, 1-2 parts of adhesion promoter, 3-6 parts of fumed silica and 1-3 parts of blue color paste. By developing a new formula system, the polyvinyl acetate emulsion is synthesized by emulsion polymerization, and a specific ratio of leveling agent, blue color paste, adhesion promoter and fumed silica is added to the mixed solution of polyvinyl acetate emulsion and polyvinyl alcohol aqueous solution to obtain a photosensitive emulsion with high adhesion, which effectively improves the adhesion of the photosensitive emulsion on the steel wire mesh of the printing screen, thereby avoiding cracking and explosion of the printing screen and improving the service life of the printing screen. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] The embodiment of the present invention provides a photosensitive emulsion for printing screen, comprising the following components in parts by weight:
[0026]
[0027] Optionally, based on the weight of each raw material component, the polyvinyl acetate emulsion includes 4 to 6 parts of polyvinyl alcohol, 50 to 60 parts of deionized water, 0.5 to 1 part of a surfactant, 303 to 406 parts of monomer vinyl acetate, 0.53 to 1.06 parts of an initiator, 1.1 to 2.2 parts of a buffer, 3 to 5 parts of acrylic acid, 50 to 70 parts of ethyl acrylate and 1 to 2 parts of dipropylene phthalate.
[0028] Alternatively, the surfactant may be, but is not limited to, Lutensol TO-7.
[0029] Alternatively, the initiator may be, but is not limited to, potassium persulfate.
[0030] Alternatively, the buffer may be, but is not limited to, sodium acetate.
[0031] Optionally, the concentration of the polyvinyl alcohol aqueous solution is 15% to 20%.
[0032] Optionally, the adhesion promoter is Easepi 516. Since the adhesion promoter Easepi 516 is an epoxy silane oligomer with a special structure, it can significantly improve the bonding strength, water resistance and corrosion resistance of the photosensitive emulsion, and can effectively improve the adhesion of the photosensitive emulsion on the steel mesh of the printing screen, thereby increasing the service life of the printing screen.
[0033] Alternatively, the fumed silica may be, but is not limited to, tackifying filler fumed silica R 972.
[0034] Optionally, based on the weight of each raw material component, the photosensitive emulsion used for printing screen also includes 0.5 to 1 part of green diazo photosensitizer solution.
[0035] The embodiment of the present invention also provides a method for preparing a photosensitive emulsion for a printing screen, comprising the following steps:
[0036] Step S01: weighing the raw materials of the components of the photosensitive emulsion for printing screen in any of the above embodiments or schemes;
[0037] Step S02: stirring and mixing the polyvinyl acetate emulsion and the polyvinyl alcohol aqueous solution to obtain a mixed solution A;
[0038] Step S03: adding a leveling agent, a blue color paste, an adhesion promoter and fumed silica to the mixed solution A, stirring and mixing, and obtaining a mixture B;
[0039] Step S04: stirring the mixture B in a disperser for 30 to 60 minutes to obtain a mixture C;
[0040] Step S05: Filter the mixture C, add a green diazo photosensitizer solution, stir evenly, and let stand to defoam, to obtain a photosensitive emulsion.
[0041] The embodiment of the present invention provides a photosensitive emulsion for a printing screen and a preparation method thereof. Compared with the prior art, the photosensitive emulsion comprises, by weight, 200 to 260 parts of polyvinyl acetate emulsion, 50 to 100 parts of polyvinyl alcohol aqueous solution, 1 to 2 parts of leveling agent, 1 to 2 parts of adhesion promoter, 3 to 6 parts of fumed silica and 1 to 3 parts of blue color paste. By developing a new formula system, the polyvinyl acetate emulsion is synthesized by emulsion polymerization, and a specific ratio of leveling agent, blue color paste, adhesion promoter and fumed silica is added to a mixed solution of the polyvinyl acetate emulsion and the polyvinyl alcohol aqueous solution to obtain a photosensitive emulsion with high adhesion, which can effectively improve the adhesion of the photosensitive emulsion on the steel wire mesh of the printing screen, thereby avoiding cracking and explosion of the printing screen and improving the service life of the printing screen.
[0042] The present invention also provides a method for preparing polyvinyl acetate emulsion by emulsion polymerization, comprising the following steps:
[0043] 1) Preparation of emulsion polymerization substrate: 4-6 parts of polyvinyl alcohol and 50-60 parts of deionized water are added to a reactor, stirred and dissolved at 90° C. for 1 hour, then cooled to 60° C., 0.5-1 parts of surfactant Lutensol TO-7, 3-6 parts of monomer vinyl acetate, 0.03-0.06 parts of initiator potassium persulfate and 0.1-0.2 parts of buffer sodium acetate are added to the reactor, and the reactants are used as emulsion polymerization substrate;
[0044] 2) Preparation of a mixed solution: adding 0.5-1 parts of an initiator potassium persulfate, 300-400 parts of a monomer vinyl acetate, 3-5 parts of acrylic acid, 50-70 parts of ethyl acrylate and 1-2 parts of dipropylene phthalate into a mixing container, and stirring to obtain a mixed solution;
[0045] 3) The reaction kettle containing the emulsion polymerization reaction substrate is heated to 80°C, and after the reflux stops, the mixed solution is added dropwise at the same time. Specifically, the mixed solution in step 2) is added dropwise within 4.5 hours, and the temperature during the reaction is maintained at 75-80°C. After the addition is completed, the temperature is kept at 80°C for 1 hour, and after cooling, 1-2 parts of sodium acetate as a buffer are added, and then the material can be discharged to obtain a polyvinyl acetate emulsion.
[0046] In order to more effectively illustrate the technical solution of the present invention, the technical solution of the present invention is described below through specific embodiments.
[0047] Example 1
[0048] 1) Preparation of emulsion polymerization reaction substrate: 4 parts of polyvinyl alcohol and 50 parts of deionized water were added to a reactor, stirred and dissolved at 90° C. for 1 hour, then cooled to 60° C., 0.5 parts of surfactant Lutensol TO-7, 3 parts of monomer vinyl acetate, 0.03 parts of initiator potassium persulfate and 0.1 parts of buffer sodium acetate were added to the reactor, and the reactants were used as emulsion polymerization reaction substrate;
[0049] 2) Preparation of a mixed solution: 0.5 parts of an initiator potassium persulfate, 300 parts of a monomer vinyl acetate, 3 parts of acrylic acid, 50 parts of ethyl acrylate and 1 part of dipropylene phthalate are added into a mixing container, and stirred to obtain a mixed solution;
[0050] 3) The reaction kettle containing the emulsion polymerization reaction substrate is heated to 80°C, and after the reflux stops, the mixed solution is added dropwise at the same time. Specifically, the mixed solution in step 2) is added dropwise within 4.5 hours, and the temperature during the reaction is maintained at 75°C. After the addition is completed, the temperature is kept at 80°C for 1 hour, and after cooling, 1 part of the buffer sodium acetate is added, and then the material can be discharged to obtain a polyvinyl acetate emulsion;
[0051] 4) 200 parts of polyvinyl acetate emulsion and 100 parts of 15% polyvinyl alcohol (PVA17-88) aqueous solution were stirred and mixed to obtain a mixed solution A1;
[0052] 5) Add 1 part of leveling agent, 1 part of blue color paste, 2 parts of adhesion promoter Easepi 516 and 6 parts of tackifying filler fumed silica R 972 to the mixed solution A1, stir and mix to obtain a mixture B1;
[0053] 6) Stirring the mixture B1 in a disperser for 30 min to obtain a mixture C1;
[0054] 7) The mixture C1 was filtered, and a green diazo photosensitizer solution was added, stirred evenly, and allowed to stand for defoaming to obtain a photosensitive emulsion D1.
[0055] Example 2
[0056] 1) Preparation of emulsion polymerization substrate: 6 parts of polyvinyl alcohol and 60 parts of deionized water were added to a reactor, stirred and dissolved at 90° C. for 1 hour, then cooled to 60° C., 1 part of surfactant Lutensol TO-7, 6 parts of monomer vinyl acetate, 0.06 parts of initiator potassium persulfate and 0.2 parts of buffer sodium acetate were added to the reactor, and the reactants were used as emulsion polymerization substrate;
[0057] 2) Preparation of a mixed solution: Add 1 part of an initiator potassium persulfate, 400 parts of a monomer vinyl acetate, 5 parts of acrylic acid, 70 parts of ethyl acrylate and 2 parts of dipropylene phthalate into a mixing container, and stir to obtain a mixed solution;
[0058] 3) The reaction kettle containing the emulsion polymerization reaction substrate is heated to 80°C, and after the reflux stops, the mixed solution is added dropwise at the same time. Specifically, the mixed solution in step 2) is added dropwise within 4.5 hours, and the temperature during the reaction is maintained at 80°C. After the addition is completed, the temperature is kept at 80°C for 1 hour, and after cooling, 2 parts of sodium acetate buffer are added, and then the material can be discharged to obtain polyvinyl acetate emulsion;
[0059] 4) 260 parts of polyvinyl acetate emulsion and 75 parts of 20% polyvinyl alcohol (PVA17-88) aqueous solution were stirred and mixed to obtain a mixed solution A2;
[0060] 5) Add 2 parts of leveling agent, 2 parts of blue color paste, 1.5 parts of adhesion promoter Easepi 516 and 3 parts of tackifying filler fumed silica R 972 to the mixed solution A2, stir and mix to obtain a mixture B2;
[0061] 6) stirring the mixture B2 in a disperser for 50 min to obtain a mixture C2;
[0062] 7) Filter the mixture C2, add the green diazo photosensitizer solution, stir evenly, and let stand to defoam, to obtain the photosensitive emulsion D2.
[0063] Example 3
[0064] 1) Preparation of emulsion polymerization substrate: 4.5 parts of polyvinyl alcohol and 55 parts of deionized water were added to a reactor, stirred and dissolved at 90° C. for 1 hour, then cooled to 60° C., 0.8 parts of surfactant Lutensol TO-7, 3.65 parts of monomer vinyl acetate, 0.04 parts of initiator potassium persulfate and 0.16 parts of buffer sodium acetate were added to the reactor, and the reactants were used as emulsion polymerization substrates;
[0065] 2) Preparation of a mixed solution: Add 0.76 parts of an initiator potassium persulfate, 360 parts of a monomer vinyl acetate, 4 parts of acrylic acid, 60 parts of ethyl acrylate and 1 part of dipropylene phthalate into a mixing container, and stir to obtain a mixed solution;
[0066] 3) The reaction kettle containing the emulsion polymerization reaction substrate is heated to 80°C, and after the reflux stops, the mixed solution is added dropwise at the same time. Specifically, the mixed solution in step 2) is added dropwise within 4.5 hours, and the temperature during the reaction is maintained at 78°C. After the addition is completed, the temperature is kept at 80°C for 1 hour, and after cooling, 1.5 parts of sodium acetate as a buffer is added, and then the material can be discharged to obtain a polyvinyl acetate emulsion;
[0067] 4) 225 parts of polyvinyl acetate emulsion and 100 parts of 18% polyvinyl alcohol (PVA17-88) aqueous solution were stirred and mixed to obtain a mixed solution A3;
[0068] 5) Add 1.5 parts of leveling agent, 2 parts of blue color paste, 1 part of adhesion promoter Easepi516 and 5 parts of tackifying filler fumed silica R 972 to the mixed solution A3, stir and mix to obtain a mixture B3;
[0069] 6) stirring the mixture B3 in a disperser for 60 min to obtain a mixture C3;
[0070] 7) The mixture C3 is filtered, and a green diazo photosensitizer solution is added, stirred evenly, and allowed to stand for defoaming to obtain a photosensitive emulsion D3.
[0071] Comparative Example 1
[0072] 1) Preparation of emulsion polymerization substrate: 4.5 parts of polyvinyl alcohol and 50 parts of deionized water were added to a reactor, stirred and dissolved at 90° C. for 1 hour, then cooled to 60° C., 0.5 parts of surfactant Lutensol TO-7, 3.65 parts of monomer vinyl acetate, 0.04 parts of initiator potassium persulfate and 0.16 parts of buffer sodium acetate were added to the reactor, and the reactants were used as emulsion polymerization substrates;
[0073] 2) Preparation of a mixed solution: Add 0.76 parts of an initiator potassium persulfate, 360 parts of a monomer vinyl acetate, 4 parts of acrylic acid, 60 parts of ethyl acrylate and 1 part of dipropylene phthalate into a mixing container, and stir to obtain a mixed solution;
[0074] 3) The reaction kettle containing the emulsion polymerization reaction substrate is heated to 80°C, and after the reflux stops, the mixed solution is added dropwise at the same time. Specifically, the mixed solution in step 2) is added dropwise within 4.5 hours, and the temperature during the reaction is maintained at 80°C. After the addition is completed, the temperature is kept at 80°C for 1 hour, and after cooling, 1.5 parts of sodium acetate as a buffer is added, and then the material can be discharged to obtain a polyvinyl acetate emulsion;
[0075] 4) 225 parts of polyvinyl acetate emulsion and 75 parts of 18% polyvinyl alcohol (PVA17-88) aqueous solution were stirred and mixed to obtain a mixed solution A4;
[0076] 5) Add 1.5 parts of leveling agent, 1.5 parts of blue color paste and 3 parts of fumed silica R972, a viscosity increasing filler, to the mixed solution A4, and stir to mix to obtain a mixture B4;
[0077] 6) stirring the mixture B4 in a disperser for 60 min to obtain a mixture C4;
[0078] 7) Filter the mixture C4, add the green diazo photosensitizer solution, stir evenly, and let stand to defoam, to obtain the photosensitive emulsion D4.
[0079] First, the photosensitive emulsions D1, D2, D3, and D4 prepared for printing screens in Examples 1 to 3 and Comparative Examples 1 to 3 were used to make four main grid screens, and the four main grid screens were numbered E1, E2, E3, and E4, respectively, and the number of printing times (service life) at which the four main grid screens began to crack and explode were tested. The relevant performance test results are listed in the following Table 1.
[0080] Table 1 Test results of photosensitive emulsions used for printing screens in Examples 1 to 3 and Comparative Example 1
[0081] Test items Main grid plate number Number of prints (10,000 times) Example 1 <![CDATA[E1]]> 10.5 Example 2 <![CDATA[E2]]> 10.5 Example 3 <![CDATA[E3]]> 10.5 Comparative Example 1 <![CDATA[E4]]> 9.5
[0082] Through the analysis of Table 1 above, it can be seen that compared with the busbar screen plate in Comparative Example 1, the number of printing times when the busbar screen plates in Examples 1 to 3 begin to crack and explode is much greater than the number of printing times when the busbar screen plates in Comparative Example 1 begin to crack and explode, that is, the service life of the busbar screen plates in Examples 1 to 3 is significantly higher than the service life of the busbar screen plates in Comparative Example 1. This indicates that the photosensitive emulsions used for printing screens in Examples 1 to 3 are significantly improved in adhesion compared to the photosensitive emulsions used for printing screens in Comparative Example 1, and the stability and consistency of adhesion are better.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A photosensitive emulsion for printing screen, characterized in that: The composition comprises the following components in parts by weight:
2. The photosensitive emulsion for printing screen according to claim 1, characterized in that: According to the weight parts of each raw material component, the polyvinyl acetate emulsion includes 4 to 6 parts of polyvinyl alcohol, 50 to 60 parts of deionized water, 0.5 to 1 part of surfactant, 303 to 406 parts of monomer vinyl acetate, 0.53 to 1.06 parts of initiator, 1.1 to 2.2 parts of buffer, 3 to 5 parts of acrylic acid, 50 to 70 parts of ethyl acrylate and 1 to 2 parts of dipropylene phthalate.
3. The photosensitive emulsion for printing screen according to claim 2, characterized in that: The surfactant is Lutensol TO-7.
4. The photosensitive emulsion for printing screen according to claim 2, characterized in that: The initiator is potassium persulfate.
5. The photosensitive emulsion for printing screen according to claim 2, characterized in that: The buffer is sodium acetate.
6. The photosensitive emulsion for printing screen according to claim 1, characterized in that: The concentration of the polyvinyl alcohol aqueous solution is 15% to 20%.
7. The photosensitive emulsion for printing screen according to claim 1, characterized in that: The adhesion promoter is Easepi 516.
8. The photosensitive emulsion for printing screen according to claim 1, characterized in that: The fumed silica is fumed silica R 972, a viscosity-enhancing filler.
9. The photosensitive emulsion for printing screen according to any one of claims 1 to 8, characterized in that: According to the weight of each raw material component, the photosensitive emulsion for printing screen also includes 0.5 to 1 part of green diazo photosensitizer solution.
10. A method for preparing a photosensitive emulsion for printing screen, characterized in that: The steps include: Step S01: Weighing the raw materials of the components of the photosensitive emulsion for printing screen according to any one of claims 1 to 9; Step S02: stirring and mixing the polyvinyl acetate emulsion and the polyvinyl alcohol aqueous solution to obtain a mixed solution A; Step S03: adding a leveling agent, a blue color paste, an adhesion promoter and fumed silica to the mixed solution A, stirring and mixing, to obtain a mixture B; Step S04: stirring the mixture B in a disperser for 30 to 60 minutes to obtain a mixture C; Step S05: Filter the mixture C, add a green diazo photosensitizer solution, stir evenly, and let stand to defoam, to obtain a photosensitive emulsion.
Citation Information
Patent Citations
Water soluble polymer mixed emulsion, coating and preparation method thereof
CN102127277A
Method for preparing polyvinyl acetate adhesive
CN108753218A
Benzene-free high-weather-proof water-based adhesive and preparation method thereof
CN109233700A
Bio-based water-resistant photosensitive adhesive as well as preparation method and application thereof