Composite material for automotive exterior parts using PCR material and method for preparing same

Through the composite material of modified polypropylene and modified hollow glass microspheres, the problem of insufficient mechanical properties and UV aging resistance in automotive exterior parts after consumption is solved, and the mechanical properties of the material are improved and The interface interaction is enhanced and suitable for automotive exterior parts.

CN119081334AInactive Publication Date: 2024-12-06CHONGQING GUANGYA POLYMER NEW MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411329867.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When using post-consumer recycling of polypropylene materials as composite material matrix, there are problems such as degradation of mechanical properties, poor resistance to UV aging, and insufficient interface bonding between fillers and substrates, which affects its application in automotive exterior parts.

Method used

Using a composite material of modified polypropylene and modified hollow glass microspheres, the polyfunctional double bond phenyltriaminotriazine anti-ultraviolet agent is introduced into polypropylene to cross-link to form a microgel with ultraviolet resistance. , and surface modification is performed on the surface of hollow glass microspheres to form chemical bond connections to enhance interface interactions and form microcrosslinked structures.

Benefits of technology

It significantly improves the mechanical properties, UV aging resistance and melt viscosity of the composite material, and improves its applicability as a material for automotive exterior parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081334A_ABST
    Figure CN119081334A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material using a PCR material for automobile exterior trimming parts and a preparation method of the composite material, and relates to the technical field of high polymer materials. The composite material using the PCR material for the automobile exterior trimming part comprises modified polypropylene and modified hollow glass microspheres, the modified polypropylene comprises polypropylene cross-linked by a cross-linking agent, the structural formula of the cross-linking agent is shown as the following formula: # imgabs 0 # modified hollow glass microspheres comprise hollow glass microspheres and modified groups connected to the surfaces of the hollow glass microspheres, the structural formula of the modified groups is shown as the following formula: # imgabs 1 #, and m is an integer of 50-100. The composite material using the PCR material for the automobile exterior trimming parts, provided by the invention, has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to a composite material for automobile exterior parts using PCR materials and a preparation method thereof. Background Art

[0002] With the continuous advancement of modernization, plastic products play an important role in our daily lives. However, the sharp increase in plastic waste has caused severe challenges to the environment and resources. In order to solve this problem, it is necessary to find a feasible way to reduce the impact of waste plastics on the environment and achieve sustainable resource utilization. Post-Consumer Recycled Material (PCR) is a type of plastic, which usually refers to waste plastics generated during the circulation, consumption and use of plastics, such as PET (polyethylene terephthalate), PP (polypropylene), HDPE (high-density polyethylene), etc. Through physical or chemical recycling, the plastic raw materials used to make new packaging materials are reprocessed and converted into valuable industrial production raw materials. The application of PCR materials is not only environmentally friendly and realizes the recycling of resources, but also has economic benefits, provides a sustainable development option, and promotes the development of the waste plastic recycling industry.

[0003] In the related art, when post-consumer recycled polypropylene materials are used as the matrix of composite materials, due to the aging and degradation of plastic products during use and the reduction of molecular weight, PCR materials have the disadvantages of reduced mechanical properties, decreased resistance to UV aging, reduced melt viscosity, and poor composite ability with fillers compared to unused materials.

[0004] Hollow glass microspheres are a type of filler with good thermal stability, corrosion resistance, and the ability to reduce the density and shrinkage of composite materials. The composite materials prepared by melt blending with polypropylene have the advantages of light weight and high strength, and are widely used in the manufacture of automotive structural parts, interior and exterior trims, and other parts. However, the interfacial bonding between hollow glass microspheres and polymer matrices is poor, and it is usually necessary to use silane coupling agents to modify the surface of hollow glass microspheres before compounding with the polymer matrix. The toughness of the prepared composite materials is still significantly reduced. Summary of the invention

[0005] In view of this, the present application provides a composite material for automobile exterior parts using PCR material and a preparation method thereof.

[0006] The embodiment of the present application is implemented as follows: a composite material for automobile exterior parts using PCR material, including modified polypropylene and modified hollow glass microspheres;

[0007] Modified polypropylene includes polypropylene cross-linked by a cross-linking agent, and the structural formula of the cross-linking agent is shown as follows:

[0008]

[0009] The modified hollow glass microspheres include hollow glass microspheres and modified groups connected to the surface of the hollow glass microspheres. The structural formula of the modified groups is shown below:

[0010]

[0011] Here, m is an integer from 50 to 100.

[0012] Optionally, in some embodiments of the present application, in the composite material for automobile exterior parts using PCR material, the mass ratio of modified polypropylene to modified hollow glass microspheres is (50-90): (10-50); and / or

[0013] The modified polypropylene and the modified hollow glass microspheres are connected by chemical bonds; and / or

[0014] The modified polypropylene and the modified hollow glass microspheres form a cross-linked structure; and / or

[0015] The polypropylene is PCR polypropylene; and / or

[0016] In the modified group, m is an integer of 50 to 100; and / or

[0017] The modified hollow glass microspheres are of core-shell structure, the core layer material of the core-shell structure is the hollow glass microspheres, and the shell layer material of the core-shell structure is the modified group.

[0018] Optionally, in some embodiments of the present application, the composite material further comprises one or more of a first grafting initiator and an antioxidant;

[0019] Optionally, the first grafting initiator comprises a peroxide, and the peroxide is selected from one or more of dicumyl peroxide, benzoyl peroxide and diacetyl peroxide;

[0020] Optionally, the antioxidant is selected from one or more of antioxidant 412S, antioxidant 1010 and antioxidant AO-1010;

[0021] Optionally, the mass ratio of the first grafting initiator to the modified hollow glass microspheres is (0.2-0.8): (10-50);

[0022] Optionally, the mass ratio of the antioxidant to the modified hollow glass microspheres is (0.2-0.8): (10-50).

[0023] Accordingly, the present application also provides a method for preparing a composite material for automotive exterior parts using PCR material, comprising the following steps:

[0024] Modified polypropylene and modified hollow glass microspheres are provided. The modified polypropylene includes polypropylene cross-linked by a cross-linking agent. The structural formula of the cross-linking agent is shown as follows: The modified hollow glass microspheres include hollow glass microspheres and modified groups connected to the surface of the hollow glass microspheres. The structural formula of the modified groups is shown below:

[0025] Wherein, m is an integer from 50 to 100;

[0026] The modified polypropylene and the modified hollow glass microspheres are mixed and reacted to obtain a composite material for automobile exterior parts using PCR material.

[0027] Optionally, in some embodiments of the present application, the method for preparing modified polypropylene includes:

[0028] Providing a 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, wherein the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion comprises 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and a first solvent;

[0029] Providing acryloyl chloride, mixing acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, reacting to obtain a crosslinking agent;

[0030] Providing polypropylene, mixing the polypropylene and a cross-linking agent, and reacting them to obtain modified polypropylene.

[0031] Optionally, in some embodiments of the present application, the molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to acryloyl chloride is 1:(3-5); and / or

[0032] The mass ratio of polypropylene to cross-linking agent is (95-99): (1-5);

[0033] The mixing reaction of acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion is carried out in an ice bath; and / or

[0034] The time for mixing the acryloyl chloride and the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion is 1.5 h to 4 h;

[0035] The mixing reaction of polypropylene and the cross-linking agent includes a first internal kneading; the temperature of the first internal kneading is 180° C. to 250° C., the time is 5 min to 20 min, and the rotation speed is 30 rpm to 100 rpm.

[0036] Optionally, in some embodiments of the present application, the method for preparing the modified hollow glass microspheres comprises:

[0037] Providing an alkaline solution and hollow glass microspheres, wherein the alkaline solution includes an alkali and a second solvent; mixing the alkaline solution and the hollow glass microspheres, reacting, and obtaining an intermediate product, wherein the intermediate product is the hollow glass microspheres and hydroxyl groups connected to the surface of the hollow glass microspheres;

[0038] Providing a PDMS dispersion and ethyl isocyanate acrylate, wherein the PDMS dispersion includes PDMS and a third solvent; mixing the PDMS dispersion and the ethyl isocyanate acrylate, reacting, and obtaining a first modified PDMS;

[0039] Providing a first modified PDMS dispersion and hexamethylene diisocyanate, wherein the first modified PDMS dispersion includes a first modified PDMS and a fourth solvent; mixing the first modified PDMS dispersion and hexamethylene diisocyanate, reacting, and obtaining a second modified PDMS;

[0040] An intermediate product dispersion is provided, wherein the intermediate product dispersion comprises an intermediate product and a fifth solvent; the intermediate product dispersion is mixed with a second modified PDMS to react and obtain modified hollow glass microspheres.

[0041] Optionally, in some embodiments of the present application, the structural formula of the first modified PDMS is as shown below: wherein m is an integer from 50 to 100; and / or

[0042] The structural formula of the second modified PDMS is shown below:

[0043]

[0044] wherein m is an integer from 50 to 100; and / or

[0045] The base includes one or more of sodium hydroxide, potassium hydroxide, and magnesium hydroxide; and / or

[0046] The molar ratio of PDMS to ethyl isocyanate acrylate is (1-1.05):1; and / or

[0047] The molar ratio of the first modified PDMS to hexamethylene diisocyanate is 1:(1-1.05); and / or the temperature of the mixed reaction of the alkali solution and the hollow glass microspheres is 60° C. to 100° C., and the time is 2 h to 5 h; and / or

[0048] The temperature of the mixed reaction of the PDMS dispersion and ethyl isocyanate acrylate is 50° C. to 80° C. and the time is 2 h to 5 h; and / or

[0049] The temperature of the mixed reaction of the first modified PDMS dispersion and hexamethylene diisocyanate is 50° C. to 80° C. and the time is 2 h to 5 h; and / or

[0050] The temperature of the mixed reaction of the intermediate product dispersion and the second modified PDMS is 40° C. to 80° C., and the time is 8 h to 15 h.

[0051] Optionally, in some embodiments of the present application, the mass ratio of modified polypropylene to modified hollow glass microspheres is (50-90): (10-50);

[0052] The modified polypropylene and the modified hollow glass microspheres are mixed and further include adding one or more of a first grafting initiator and an antioxidant;

[0053] The modified polypropylene and the modified hollow glass microspheres are mixed and reacted, and the second mixing is performed at a temperature of 180°C to 250°C, a time of 5min to 20min, and a rotation speed of 30rpm to 100rpm.

[0054] Correspondingly, an embodiment of the present application further provides an automobile exterior trim, the material of which includes the above-mentioned composite material, or includes the composite material prepared by the above-mentioned preparation method.

[0055] The composite material for automobile exterior parts using PCR material provided in the present application adopts a phenyltriaminotriazine anti-ultraviolet agent containing multifunctional double bonds as a cross-linking agent to cross-link polypropylene, and the formation of a "microgel with anti-ultraviolet ability" structure improves the mechanical properties, anti-ultraviolet aging properties, melt viscosity, etc. of the modified polypropylene material to a level that can be directly used as a matrix material; hollow glass microspheres are selected as low-density reinforcing fillers, and the modified groups on the surface enable the modified hollow glass microspheres to effectively enhance and toughen the modified polypropylene matrix; by forming chemical bonds between the modified hollow glass microspheres and the modified polypropylene matrix, the interface interaction between the two is enhanced; at the same time, the rich reactive groups on the surface of the modified hollow glass microspheres enable the modified polypropylene / modified hollow glass microsphere composite material to form a micro-cross-linked structure, further improving the mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0057] Figure 1 This is a flow chart of a method for preparing a composite material for automotive exterior parts using PCR material provided in an embodiment of the present application. DETAILED DESCRIPTION

[0058] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0059] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0060] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0061] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple, respectively.

[0062] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0063] The structural formula and molecular weight of some chemical reagents used in this application are described as follows:

[0064] 2,4,6-Tris(4-aminophenyl)-1,3,5-triazine: Molecular weight = 354.41;

[0065] Acryloyl chloride: CH2=CH-COCl, molecular weight = 90.51;

[0066] Hydroxyl-terminated polydimethylsiloxane (PDMS): m represents the degree of polymerization of PDMS, which is an integer of 50-150.

[0067] The technical solution of this application is as follows:

[0068] In a first aspect, an embodiment of the present application provides a composite material for automotive exterior parts using PCR material, the composite material comprising modified polypropylene and modified hollow glass microspheres;

[0069] Modified polypropylene includes polypropylene cross-linked by a cross-linking agent, and the structural formula of the cross-linking agent is shown as follows:

[0070]

[0071] The modified hollow glass microspheres include hollow glass microspheres and modified groups connected to the surface of the hollow glass microspheres. The structural formula of the modified groups is shown below:

[0072]

[0073] Here, m is an integer from 50 to 100.

[0074] It should be noted that in this application, = represents the degree of polymerization of -R- as x, in other words, x represents the number of monomer repeating units in the polymer chain. Similarly, Indicates the thermoplastic elastomer The number of repetitions is m, specifically 50 to 100.

[0075] It should be noted that, in the present application, the "*" in *——R represents a connection site.

[0076] It should also be noted that hollow glass microspheres are specially processed glass microspheres, which are characterized by lower density and poorer thermal conductivity than glass microspheres. Hollow glass microspheres are a new type of micron-sized lightweight material, whose main component is borosilicate, and have the characteristics of high compressive strength, high melting point, high resistivity, small thermal conductivity and thermal shrinkage coefficient.

[0077] The composite material for automobile exterior parts using PCR material provided in the present application adopts a phenyltriaminotriazine anti-ultraviolet agent containing multifunctional double bonds as a cross-linking agent to cross-link polypropylene, and the formation of a "microgel with anti-ultraviolet ability" structure improves the mechanical properties, anti-ultraviolet aging properties, melt viscosity, etc. of the modified polypropylene material to a level that can be directly used as a matrix material; hollow glass microspheres are selected as low-density reinforcing fillers, and the modified groups on the surface enable the modified hollow glass microspheres to effectively enhance and toughen the modified polypropylene matrix; by forming chemical bonds between the modified hollow glass microspheres and the modified polypropylene matrix, the interface interaction between the two is enhanced; at the same time, the rich reactive groups on the surface of the modified hollow glass microspheres enable the modified polypropylene / modified hollow glass microsphere composite material to form a micro-cross-linked structure, further improving the mechanical properties of the composite material.

[0078] In some embodiments, the polypropylene is PCR polypropylene. In other words, the polypropylene is post-consumer recycled polypropylene.

[0079] In some embodiments, in the modified group, m can be selected from integers of 55 to 95, integers of 60 to 90, integers of 70 to 80, etc. Specifically, m can be 58, 62, 66, 75, 85, 88, 97, etc.

[0080] In some embodiments, the modified hollow glass microspheres are core-shell structures, the core layer material of the core-shell structure is hollow glass microspheres, and the shell layer material of the core-shell structure is a modified group. In the core-shell structure, the unique "rigid core + elastic shell" structure enables the modified hollow glass microspheres to effectively enhance and toughen the post-consumer recycled polypropylene matrix.

[0081] In some embodiments, in the composite material for automobile exterior parts using PCR material, the mass ratio of modified polypropylene to modified hollow glass microspheres is (50-90): (10-50), for example, 50:50, 60:40, 70:30, 80:20, 90:10, etc. Within the mass ratio range, the modified polypropylene and the modified hollow glass microspheres are conducive to synergistic effect, and the mechanical properties of the composite material are jointly improved.

[0082] In some embodiments, in the composite material, the modified polypropylene and the modified hollow glass microspheres are connected by chemical bonds.

[0083] In some embodiments, in the composite material, the modified polypropylene and the modified hollow glass microspheres form a cross-linked structure.

[0084] In some embodiments, the composite material further includes one or more of a first grafting initiator and an antioxidant.

[0085] In some embodiments, the first grafting initiator comprises a peroxide, and the peroxide is selected from one or more of dicumyl peroxide, benzoyl peroxide, and diacetyl peroxide.

[0086] In some embodiments, the antioxidant is selected from one or more of Antioxidant 412S, Antioxidant 1010, and Antioxidant AO-1010.

[0087] In some embodiments, the mass ratio of the first grafting initiator to the modified hollow glass microspheres is (0.2-0.8):(10-50), for example, 0.3:40, 0.4:35, 0.5:30, 0.6:25, 0.7:20, etc. Within the mass ratio range, the first grafting initiator is beneficial to promote the connection between the modified polypropylene and the modified hollow glass microspheres.

[0088] In some embodiments, the mass ratio of the antioxidant to the modified hollow glass microspheres is (0.2-0.8):(10-50), for example, 0.3:40, 0.4:35, 0.5:30, 0.6:25, 0.7:20, etc. Within the mass ratio range, it is beneficial to improve the antioxidant properties of the composite material.

[0089] In some embodiments, the composite material for automobile exterior parts using PCR material consists of modified polypropylene, modified hollow glass microspheres, a first grafting initiator, and an antioxidant.

[0090] Second, see Figure 1 The present application also provides a method for preparing a composite material for automobile exterior parts using PCR material, comprising the following steps:

[0091] S11. Provide modified polypropylene and modified hollow glass microspheres, wherein the modified polypropylene includes polypropylene cross-linked by a cross-linking agent, and the structural formula of the cross-linking agent is as follows: The modified hollow glass microspheres include hollow glass microspheres and modified groups connected to the surface of the hollow glass microspheres. The structural formula of the modified groups is shown below:

[0092] Wherein, m is an integer from 50 to 100;

[0093] S12, mixing the modified polypropylene and the modified hollow glass microspheres, reacting them, and obtaining a composite material for automobile exterior parts using PCR material.

[0094] In S11:

[0095] In some embodiments, the method for preparing modified polypropylene comprises:

[0096] S111, providing a 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, wherein the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion comprises 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and a first solvent;

[0097] S112, providing acryloyl chloride, mixing acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, reacting to obtain a crosslinking agent;

[0098] S113, providing polypropylene, mixing the polypropylene and the cross-linking agent, reacting, and obtaining modified polypropylene.

[0099] In S111:

[0100] In some embodiments, in the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, the molar concentration of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine is 0.05 mmol / mL to 0.2 mmol / mL, for example, 0.06 mmol / mL, 0.08 mmol / mL, 0.1 mmol / mL, 0.15 mmol / mL, 0.18 mmol / mL, etc. Within this molar concentration range, it is beneficial to uniformly dissolve and disperse 2,4,6-tris(4-aminophenyl)-1,3,5-triazine.

[0101] In some embodiments, the first solvent is selected from one or more of toluene, n-octane, isooctane, n-hexane, cyclohexane, ethyl acetate, benzene, chloroform, carbon tetrachloride, dichloromethane, dimethyl ether, and tetraethylene glycol dimethyl ether.

[0102] In some embodiments, the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion further includes an acid binding agent.

[0103] Furthermore, the acid binding agent is selected from one or more of triethylamine and pyridine.

[0104] In the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, the mass ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to the acid-binding agent is (1-3):1, for example, 1.2:1, 1.5:1, 1.8:1, 2:1, 2.2:1, 2.5:1, 2.8:1, etc. Within the mass ratio range, the reaction of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and acryloyl chloride is promoted, and the reaction efficiency is improved.

[0105] In S112:

[0106] In some embodiments, the molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to acryloyl chloride is 1:(3-5), for example, 1:3.5, 1:4, 1:4.5, etc. Within the range of this mass ratio, the reaction efficiency of acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine is improved.

[0107] In some embodiments, the mixing reaction of acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion is carried out in an ice bath. The mixing reaction time of acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion is 1.5 hours to 4 hours, for example, 1.8 hours, 2 hours, 2.2 hours, 2.5 hours, 2.8 hours, 3 hours, 3.2 hours, 3.5 hours, 3.8 hours, etc. In this way, under the conditions of the reaction, it is beneficial to promote the reaction of acryloyl chloride and 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to generate a crosslinking agent.

[0108] Exemplarily, the reaction formula of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and acryloyl chloride is as follows:

[0109]

[0110] In S113:

[0111] Polypropylene can be purchased commercially, such as PCR polypropylene purchased from Blue Planet Biodegradable Materials Co., Ltd.

[0112] In some embodiments, the mass ratio of polypropylene to the crosslinking agent is (95-99):(1-5), for example, 96:4, 97:3, 98:2, etc. Within the mass ratio range, the crosslinking agent is conducive to crosslinking the polypropylene.

[0113] In some embodiments, mixing the polypropylene and the crosslinking agent further comprises adding a second grafting initiator.

[0114] Furthermore, the second grafting initiator includes a peroxide, and the peroxide is selected from one or more of dicumyl peroxide, benzoyl peroxide and diacetyl peroxide.

[0115] In some embodiments, the mass ratio of the crosslinking agent to the second grafting initiator is (1-5): (0.2-0.8), for example, 2:0.5, 3:0.5, 4:0.5, etc. Within the mass ratio range, the second grafting initiator is conducive to initiating the crosslinking of the crosslinking agent to the polypropylene to obtain modified polypropylene.

[0116] In some embodiments, the mixing reaction of the polypropylene and the cross-linking agent comprises a first internal mixing.

[0117] Further, the temperature of the first banburying is 180°C to 250°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, etc.; the time is 5min to 20min, for example, 8min, 10min, 12min, 15min, 18min, etc.; the speed is 30rpm to 100rpm, for example, 40rpm, 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, etc. In this way, under the conditions of the first banburying, it is conducive to fully modifying the polypropylene to obtain modified polypropylene with excellent mechanical properties, anti-ultraviolet aging properties, and melt viscosity.

[0118] The present application starts from the phenyltriaminotriazine anti-ultraviolet agent commonly used in polypropylene, introduces multi-functional double bonds into it through chemical structure design, and then uses it as a cross-linking agent with anti-ultraviolet ability to melt blend with PCR polypropylene, and micro-cross-links the PCR polypropylene. The formation of the "microgel with anti-ultraviolet ability" structure improves the mechanical properties, anti-ultraviolet aging properties, melt viscosity, etc. of the modified PCR polypropylene to the level that can be directly used as a matrix material.

[0119] In some embodiments, the method for preparing the modified hollow glass microspheres comprises:

[0120] S121, providing an alkali solution and hollow glass microspheres, wherein the alkali solution includes an alkali and a second solvent; mixing the alkali solution and the hollow glass microspheres, reacting to obtain an intermediate product, wherein the intermediate product is a hollow glass microsphere and a hydroxyl group connected to the surface of the hollow glass microsphere;

[0121] S122, providing a PDMS (hydroxy-terminated polydimethylsiloxane) dispersion and ethyl isocyanate acrylate, wherein the PDMS dispersion includes PDMS and a third solvent; mixing the PDMS dispersion and ethyl isocyanate acrylate, and reacting to obtain a first modified PDMS, wherein the structural formula of the first modified PDMS is as shown below:

[0122] Wherein, m is an integer from 50 to 100;

[0123] S123, providing a first modified PDMS dispersion and 1,6-hexamethylene diisocyanate, wherein the first modified PDMS dispersion includes a first modified PDMS and a fourth solvent; mixing the first modified PDMS dispersion and 1,6-hexamethylene diisocyanate, reacting to obtain a second modified PDMS, wherein the structural formula of the second modified PDMS is as follows:

[0124]

[0125] Wherein, m is an integer from 50 to 100;

[0126] S124, providing an intermediate product dispersion, wherein the intermediate product dispersion includes the intermediate product and a fifth solvent; mixing the intermediate product dispersion and the second modified PDMS, reacting to obtain modified hollow glass microspheres.

[0127] In S121:

[0128] Hollow glass microspheres can be purchased commercially, such as 3M hollow glass microspheres VS500 purchased from Shanghai Xianglan Chemical Co., Ltd.

[0129] In some embodiments, the base includes one or more of sodium hydroxide, potassium hydroxide, and magnesium hydroxide.

[0130] In some embodiments, the second solvent includes water.

[0131] In some embodiments, the molar concentration of the alkali in the alkali solution is 0.2 mol / L to 0.8 mol / L, for example, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, etc.

[0132] In some embodiments, the temperature of the mixed reaction of the alkali solution and the hollow glass microspheres is 60° C. to 100° C., for example, 70° C., 80° C., 90° C., etc., and the reaction time is 2 h to 5 h, for example, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, etc. Thus, under the reaction conditions, it is favorable for the -OH of the alkali in the alkali solution to be connected to the hollow glass microspheres.

[0133] In S122:

[0134] In some embodiments, the molar concentration of PDMS in the PDMS dispersion is 5 mmol / L to 20 mmol / L, for example, 8 mmol / L, 10 mmol / L, 12 mmol / L, 15 mmol / L, 18 mmol / L, etc. Within this molar concentration range, it is beneficial for PDMS to be uniformly dissolved and dispersed.

[0135] In some embodiments, the third solvent is selected from one or more of anhydrous tetrahydrofuran, chlorobenzene, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether, dimethyl sulfoxide, acetone, acetophenone, N,N-dimethylformamide, ethyl acetate, and pyrrole.

[0136] In some embodiments, the molar ratio of PDMS to ethyl isocyanate acrylate is (1-1.05):1, for example, 1.01:1, 1.02:1, 1.03:1, 1.04:1, 1.05:1, etc. Within the molar ratio range, it is beneficial for PDMS and ethyl isocyanate acrylate to fully react to obtain the first modified PDMS.

[0137] In some embodiments, the mixing of the PDMS dispersion and ethyl isocyanate acrylate further includes adding a first catalyst.

[0138] Further, the first catalyst includes dibutyltin dilaurate.

[0139] In some embodiments, the mass ratio of PDMS to catalyst is (2-8):0.1, for example, 3:0.1, 4:0.1, 5:0.1, 6:0.1, 7:0.1, etc. Within the mass ratio range, the catalyst is beneficial to improve the reaction efficiency of PDMS dispersion and ethyl isocyanate acrylate.

[0140] In some embodiments, the temperature of the mixed reaction of the PDMS dispersion and the isocyanate ethyl acrylate is 50°C to 80°C, for example, 55°C, 60°C, 70°C, etc.; the time is 2h to 5h, for example, 2.5h, 3h, 3.5h, 4h, 4.5h, etc. In this way, under the conditions of the reaction, it is conducive to promoting the reaction of PDMS and isocyanate ethyl acrylate to generate the first modified PDMS. The first modified PDMS is a PDMS with a hydroxyl group at one end and a carbon-carbon double bond at the other end.

[0141] Exemplarily, the reaction formula of PDMS and ethyl isocyanate acrylate is as follows:

[0142]

[0143] In S123:

[0144] In some embodiments, the molar concentration of PDMS in the first modified PDMS dispersion is 5 mmol / L to 20 mmol / L, for example, 8 mmol / L, 10 mmol / L, 12 mmol / L, 15 mmol / L, 18 mmol / L, etc. Within this molar concentration range, the first modified PDMS is facilitated to be uniformly dissolved and dispersed.

[0145] In some embodiments, the fourth solvent is selected from one or more of anhydrous tetrahydrofuran, chlorobenzene, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether, dimethyl sulfoxide, acetone, acetophenone, N,N-dimethylformamide, ethyl acetate, and pyrrole.

[0146] In some embodiments, the molar ratio of the first modified PDMS to hexamethylene diisocyanate is 1:(1-1.05), for example, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, etc. Within the molar ratio range, it is beneficial for the first modified PDMS and hexamethylene diisocyanate to fully react to obtain the second modified PDMS.

[0147] In some embodiments, the mixing of the PDMS dispersion and ethyl isocyanate acrylate further includes adding a second catalyst.

[0148] Further, the second catalyst includes dibutyltin dilaurate.

[0149] In some embodiments, the mass ratio of the first modified PDMS to the second catalyst is (2-8):0.1, for example, 3:0.1, 4:0.1, 5:0.1, 6:0.1, 7:0.1, etc. Within the mass ratio range, the catalyst is beneficial to improve the reaction efficiency of the first modified PDMS dispersion and 1,6-hexamethylene diisocyanate.

[0150] In some embodiments, the temperature of the mixed reaction of the first modified PDMS dispersion and 1,6-hexamethylene diisocyanate is 50°C to 80°C, for example, 55°C, 60°C, 70°C, etc.; the time is 2h to 5h, for example, 2.5h, 3h, 3.5h, 4h, 4.5h, etc. In this way, under the conditions of the reaction, it is conducive to promoting the reaction of the first modified PDMS and 1,6-hexamethylene diisocyanate to generate the second modified PDMS. The second modified PDMS is a PDMS with an isocyanate group at one end and a carbon-carbon double bond at the other end.

[0151] Exemplarily, the reaction formula of the first modified PDMS and 1,6-hexamethylene diisocyanate is as follows:

[0152]

[0153] In S124:

[0154] In some embodiments, in the intermediate product dispersion, the mass concentration of the intermediate product is 50 g / L to 80 g / L, for example, 55 g / L, 60 g / L, 65 g / L, 70 g / L, 75 g / L, etc. Within this mass concentration range, the intermediate product is conducive to uniform dissolution and dispersion.

[0155] In some embodiments, the fifth solvent is selected from one or more of anhydrous tetrahydrofuran, chlorobenzene, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, diethylene glycol dimethyl ether, dimethyl sulfoxide, acetone, acetophenone, N,N-dimethylformamide, ethyl acetate, and pyrrole.

[0156] In some embodiments, mixing the intermediate product dispersion and the second modified PDMS further comprises adding a third catalyst.

[0157] Further, the third catalyst includes dibutyltin dilaurate.

[0158] In some embodiments, the temperature of the mixed reaction of the intermediate product dispersion and the second modified PDMS is 40°C to 80°C, for example, 50°C, 60°C, 70°C, etc.; the time is 8h to 15h, for example, 9h, 10h, 11h, 12h, 13h, 14h, etc. Thus, under the reaction conditions, it is favorable for the second modified PDMS to react with -OH on the intermediate product to obtain a hollow glass microsphere core and an elastic shell layer covering the hollow glass microsphere core.

[0159] Exemplarily, the reaction formula of the intermediate product and the second modified PDMS is as follows:

[0160]

[0161] This application uses hollow glass microspheres as low-density reinforcing fillers, and forms an elastic shell layer on the surface of the hollow glass microspheres through surface grafting treatment. The unique "rigid core + elastic shell" structure enables the modified hollow glass microspheres to effectively enhance and toughen the post-consumer recycled polypropylene matrix.

[0162] In S12:

[0163] In some embodiments, the mass ratio of modified polypropylene to modified hollow glass microspheres is (50-90):

[0164] (10-50), for example, 50:50, 60:40, 70:30, 80:20, 90:10, etc. Within the mass ratio range, the modified polypropylene and the modified hollow glass microspheres are conducive to synergistic effect, and the mechanical properties of the composite material are jointly improved.

[0165] In some embodiments, the modified polypropylene and the modified hollow glass microspheres are mixed and further include one or more of a first grafting initiator and an antioxidant. The materials and amounts of the first grafting initiator and the antioxidant are as described above and will not be described in detail here.

[0166] In some embodiments, the mixing reaction of the modified polypropylene and the modified hollow glass microspheres includes a second internal kneading.

[0167] Further, the temperature of the second banburying is 180°C to 250°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, etc.; the time is 5min to 20min, for example, 8min, 10min, 12min, 15min, 18min, etc.; the speed is 30rpm to 100rpm, for example, 40rpm, 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, etc. In this way, under the conditions of the second banburying, it is conducive to fully combining the modified polypropylene and the modified hollow glass microspheres to obtain a composite material for automotive exterior parts using PCR materials.

[0168] The first internal kneading and the second internal kneading can be achieved by using conventional instruments and equipment in the art, such as a small torque rheometer.

[0169] In a third aspect, the embodiments of the present application further provide an application of the composite material mentioned above or the composite material prepared by the above preparation method.

[0170] Since the composite material has excellent mechanical properties, the composite material provided by the present invention is particularly suitable for automobile exterior parts.

[0171] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0172] Example 1

[0173] This embodiment provides a composite material for automobile exterior parts using PCR material, and the preparation method thereof is as follows:

[0174] Weigh 3.54g 2,4,6-tris(4-aminophenyl)-1,3,5-triazine (10mmol), 100mL toluene and 3g triethylamine (acid binder) into a 250mL three-necked flask, start stirring, and heat to 80°C to completely dissolve 2,4,6-tris(4-aminophenyl)-1,3,5-triazine. Then transfer the three-necked flask to an ice bath, keep stirring, and drop 2.7g acryloyl chloride (30mmol) into the three-necked flask. Stop the reaction after 2h. Remove the toluene in the system by rotary evaporation, and rinse with deionized water to remove the generated triethylamine hydrochloride to obtain a crosslinking agent;

[0175] 96.5 g PCR polypropylene material, 3 g of the above cross-linking agent and 0.5 g of dicumyl peroxide (initiator) were added to a medium-speed mixer, stirred and mixed at room temperature, the speed was set to 50 rpm, and the premix was taken out after mixing for 3 min. The premix was then mixed in a small torque rheometer at a mixing temperature of 200 ° C and a speed of 30 rpm. After mixing for 5 min, the material was taken out to obtain modified polypropylene;

[0176] 100 g of hollow glass microspheres and 1 L of deionized water were added to a 2 L beaker, stirred thoroughly, and allowed to stand for 2 h. The hollow glass microspheres floating on the upper layer were taken and dried in an oven at 100 ° C for 4 h. 20 g of the dried hollow glass microspheres were added to a 1 L three-necked flask, and 500 mL of a 0.5 mol / L sodium hydroxide aqueous solution was added. The mixture was refluxed and stirred at 80 ° C for 3 h. After the reaction was completed, the residual sodium hydroxide was removed by suction filtration and repeatedly rinsed with deionized water. The mixture was dried in an oven at 100 ° C for 8 h to obtain an intermediate product (hollow glass microspheres with surface hydroxyl groups).

[0177] Take 5g of terminal hydroxyl polydimethylsiloxane (PDMS, 1mmol) and 100mL of anhydrous tetrahydrofuran and add them to a 500mL three-necked flask, heat to 60°C to completely dissolve the PDMS; then drop 0.141g of isocyanate ethyl acrylate (1mmol) and 0.1g of dibutyltin dilaurate (catalyst) into the three-necked flask, keep stirring, react at 60°C for 4h in a nitrogen atmosphere to obtain a first THF solution system of the first modified PDMS (PDMS with a hydroxyl group at one end and a carbon-carbon double bond at the other end); drop 0.168g of 1,6-hexamethylene diisocyanate (1mmol) into the solution system, keep stirring, react at 60°C for 4h in a nitrogen atmosphere to obtain a second THF solution system of the second modified PDMS (PDMS with an isocyanate group at one end and a carbon-carbon double bond at the other end);

[0178] 20 g of the intermediate product and 300 mL of anhydrous THF were added to a 500 mL three-necked flask, and ultrasonically treated at 60° C. for 2 h to obtain an intermediate product dispersion, and then the second solution system was added to the intermediate product dispersion, and stirred under a nitrogen atmosphere at 60° C. for 12 h. After the reaction was completed, the unreacted PDMS was removed by suction filtration and rinsed with excess THF, and dried in an oven at 80° C. for 4 h to obtain modified hollow glass microspheres (hollow glass microspheres with an elastic shell layer);

[0179] Repeat the above steps to prepare sufficient modified polypropylene and modified hollow glass microspheres;

[0180] 89 g of modified polypropylene, 10 g of modified hollow glass microspheres, 0.5 g of diisopropylbenzene peroxide (grafting initiator) and 0.5 g of antioxidant 412S were added to a high-speed mixer, stirred and mixed at room temperature, the speed was set to 150 rpm, and the premix was taken out after mixing for 5 minutes; the premix was then mixed in a small torque rheometer at a mixing temperature of 200°C and a speed of 30 rpm. The material was taken out after mixing for 5 minutes to obtain a composite material for automotive exterior parts using PCR materials.

[0181] Example 2

[0182] This embodiment is substantially the same as Embodiment 1, except that the composite material in this embodiment includes 79 g of modified polypropylene, 20 g of modified hollow glass microspheres, 0.5 g of diisopropylbenzene peroxide, and 0.5 g of antioxidant 412S.

[0183] Example 3

[0184] This embodiment is substantially the same as Embodiment 1, except that the composite material in this embodiment includes 69 g of modified polypropylene, 30 g of modified hollow glass microspheres, 0.5 g of dicumyl peroxide, and 0.5 g of antioxidant 412S.

[0185] Example 4

[0186] This embodiment is substantially the same as Embodiment 1, except that the composite material in this embodiment includes 59 g of modified polypropylene, 40 g of modified hollow glass microspheres, 0.5 g of dicumyl peroxide, and 0.5 g of antioxidant 412S.

[0187] Comparative Example

[0188] This comparative example is basically the same as Example 1, except that the composite material in this example includes 78g of impact-resistant copolymer PP (PP K8003, purchased from Shanghai Secco Petrochemical Co., Ltd.), 20g of unmodified hollow glass microspheres, 1.5g of silane coupling agent KH550 and 0.5g of antioxidant 412S.

[0189] The composite materials for automobile exterior parts using PCR materials of Examples 1 to 4 and the composite materials of the comparative example were hot pressed at a hot pressing temperature of 210°C and a holding time of 8 minutes, and a cold pressing temperature of 25°C and a holding time of 3 minutes to obtain specimens. The mechanical properties of the specimens were measured, and the results are shown in Table 1.

[0190] Among them, the tensile strength at break test at 50mm / min is carried out in accordance with standard GB / T1040; the bending modulus at 2.0mm / min is carried out in accordance with standard GB / T9341; and the simply supported beam notched impact test at 23°C is carried out in accordance with standard GB / T1043.

[0191] Table 1

[0192]

[0193] As can be seen from Table 1, in Examples 1 to 4, the tensile strength, flexural modulus and notched impact strength of the composite materials for automotive exterior parts using PCR materials provided by the present application are much higher than those of the composite materials in the comparative examples, among which Example 3 has the largest tensile strength, Example 4 has the largest flexural modulus, and Example 1 has the largest notched impact strength. In summary, the composite materials for automotive exterior parts using PCR materials provided by the present application have excellent mechanical properties.

[0194] The technical solutions provided by the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A composite material for automobile exterior parts using PCR material, characterized in that: Including modified polypropylene and modified hollow glass microspheres; The modified polypropylene includes polypropylene cross-linked by a cross-linking agent, and the structural formula of the cross-linking agent is shown as follows: The modified hollow glass microspheres include hollow glass microspheres and modified groups connected to the surface of the hollow glass microspheres. The structural formula of the modified groups is shown below: Here, m is an integer from 50 to 100.

2. The composite material according to claim 1, characterized in that In the composite material for automobile exterior parts using PCR material, the mass ratio of the modified polypropylene to the modified hollow glass microspheres is (50-90): (10-50); and / or The modified polypropylene and the modified hollow glass microspheres are connected by chemical bonds; and / or The modified polypropylene and the modified hollow glass microspheres form a cross-linked structure; and / or The polypropylene is PCR polypropylene; and / or In the modified group, m is an integer of 50 to 100; and / or The modified hollow glass microsphere is a core-shell structure, the core layer material of the core-shell structure is the hollow glass microsphere, and the shell layer material of the core-shell structure is the modified group.

3. The composite material according to claim 1, characterized in that The composite material further includes one or more of a first grafting initiator and an antioxidant; Optionally, the first grafting initiator comprises a peroxide, and the peroxide is selected from one or more of dicumyl peroxide, benzoyl peroxide and diacetyl peroxide; Optionally, the antioxidant is selected from one or more of antioxidant 412S, antioxidant 1010 and antioxidant AO-1010; Optionally, the mass ratio of the first grafting initiator to the modified hollow glass microsphere is (0.2-0.8): (10-50); Optionally, the mass ratio of the antioxidant to the modified hollow glass microspheres is (0.2-0.8):(10-50).

4. A method for preparing a composite material for automobile exterior parts using PCR material, characterized in that: The steps include: Modified polypropylene and modified hollow glass microspheres are provided, wherein the modified polypropylene includes polypropylene cross-linked by a cross-linking agent, and the structural formula of the cross-linking agent is shown as follows: The modified hollow glass microspheres include hollow glass microspheres and modified groups connected to the surface of the hollow glass microspheres, and the structural formula of the modified groups is shown below: Wherein, m is an integer from 50 to 100; The modified polypropylene and the modified hollow glass microspheres are mixed and reacted to obtain a composite material for automobile exterior parts using PCR material.

5. The preparation method according to claim 4, characterized in that: The preparation method of the modified polypropylene comprises: Providing a 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, wherein the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion comprises 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and a first solvent; Providing acryloyl chloride, mixing the acryloyl chloride and the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion, reacting to obtain a crosslinking agent; Providing polypropylene, mixing the polypropylene and the cross-linking agent, and reacting them to obtain modified polypropylene.

6. The preparation method according to claim 5, characterized in that: The molar ratio of the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to the acryloyl chloride is 1:(3-5); and / or The mass ratio of the polypropylene to the cross-linking agent is (95-99): (1-5); The mixing reaction of the acryloyl chloride and the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion is carried out in an ice bath; and / or The mixing reaction time of the acryloyl chloride and the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine dispersion is 1.5h to 4h; The mixing reaction of the polypropylene and the cross-linking agent includes a first banburying; the first banburying temperature is 180° C. to 250° C., the time is 5 min to 20 min, and the rotation speed is 30 rpm to 100 rpm.

7. The preparation method according to claim 4, characterized in that: The preparation method of the modified hollow glass microspheres comprises: Providing an alkali solution and hollow glass microspheres, wherein the alkali solution includes an alkali and a second solvent; mixing the alkali solution and the hollow glass microspheres, reacting to obtain an intermediate product, wherein the intermediate product is the hollow glass microspheres and hydroxyl groups connected to the surface of the hollow glass microspheres; Providing a PDMS dispersion and ethyl isocyanate acrylate, wherein the PDMS dispersion comprises PDMS and a third solvent; mixing the PDMS dispersion and the ethyl isocyanate acrylate, reacting to obtain a first modified PDMS; Providing a first modified PDMS dispersion and hexamethylene diisocyanate, wherein the first modified PDMS dispersion includes the first modified PDMS and a fourth solvent; mixing the first modified PDMS dispersion and the hexamethylene diisocyanate, reacting them, and obtaining a second modified PDMS; Providing an intermediate product dispersion, wherein the intermediate product dispersion comprises the intermediate product and a fifth solvent; mixing the intermediate product dispersion and the second modified PDMS, reacting to obtain modified hollow glass microspheres.

8. The preparation method according to claim 7, characterized in that: The structural formula of the first modified PDMS is shown below: wherein m is an integer from 50 to 100; and / or The structural formula of the second modified PDMS is shown below: wherein m is an integer from 50 to 100; and / or The alkali comprises one or more of sodium hydroxide, potassium hydroxide and magnesium hydroxide; and / or The molar ratio of the PDMS to the isocyanate ethyl acrylate is (1-1.05):1; and / or The molar ratio of the first modified PDMS to the 1,6-hexamethylene diisocyanate is 1:(1-1.05); and / or The temperature of the mixed reaction of the alkali solution and the hollow glass microspheres is 60° C. to 100° C., and the time is 2 h to 5 h; and / or The temperature of the mixed reaction of the PDMS dispersion and the isocyanate ethyl acrylate is 50° C. to 80° C. and the time is 2 h to 5 h; and / or The temperature of the mixed reaction of the first modified PDMS dispersion and the 1,6-hexamethylene diisocyanate is 50° C. to 80° C., and the time is 2 h to 5 h; and / or The temperature for the mixed reaction of the intermediate product dispersion and the second modified PDMS is 40° C. to 80° C., and the time is 8 h to 15 h.

9. The preparation method according to claim 4, characterized in that: The mass ratio of the modified polypropylene to the modified hollow glass microspheres is (50-90): (10-50); The mixing of the modified polypropylene and the modified hollow glass microspheres further includes adding one or more of a first grafting initiator and an antioxidant; The mixed reaction of the modified polypropylene and the modified hollow glass microspheres includes a second banburying; the temperature of the second banburying is 180° C. to 250° C., the time is 5 min to 20 min, and the rotation speed is 30 rpm to 100 rpm.

10. An automobile exterior trim, characterized in that: The material of the automobile exterior trim comprises the composite material as claimed in any one of claims 1 to 3, or comprises the composite material prepared by the preparation method as claimed in any one of claims 4 to 9.

Citation Information

Patent Citations

  • Hollow glass microsphere surface modification method, low density and high weather resistant polypropylene composite material and preparation method thereof

    CN109535432A

  • Preparation method of hollow glass bead master batch

    CN117567814A

  • Thermoplastic resin composite containing hollow glass microsheres

    US20140088244A1