Bio-based unsaturated polyester resin applied to mould pressing composite material of air deflector of new energy automobile

By using a combination of bio-based unsaturated polyester resin and specific additives in the shroud material, the shortcomings of existing materials in toughness, durability and environmental protection are solved, and the stability of shroud materials of new energy vehicles is significantly improved. The performance and mechanical properties meet the high requirements for materials in the new energy vehicle industry.

CN119081335APending Publication Date: 2024-12-06ZHENJIANG LEADER COMPOSITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210743.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing shroud materials have shortcomings in toughness, durability and environmental protection, especially when the new energy vehicle industry has higher requirements for the material's pressure resistance and environmental protection, the performance of existing unsaturated polyester resins insufficient.

Method used

Using bio-based unsaturated polyester resin, a specific synthetic process is carried out through the combination of unsaturated dibasic acid, diol, styrene, polymerization inhibitor, catalyst, modified filler, nanotitanium dioxide and additives, and prepared by combining unsaturated dibasic acid, diol, styrene, polyester inhibitor, catalyst, modified filler, nanotitanium dioxide and additives. Polyester resins with improved stability and durability are produced, combined with a combination of epoxidized castor oil and carbon nanotubes to enhance mechanical properties and impact strength.

Benefits of technology

It significantly improves the stability and durability of the shroud material of new energy vehicle, improves mechanical properties and impact resistance, and at the same time enhances the environmental protection of the material, meeting the high requirements for materials in the new energy vehicle industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020258360000101
    Figure BDA0005020258360000101
  • Figure BDA0005020258360000111
    Figure BDA0005020258360000111
Patent Text Reader

Abstract

The invention belongs to the technical field of polyester resin, and discloses bio-based unsaturated polyester resin applied to a mold pressing composite material of a new energy automobile fairing. The bio-based unsaturated polyester resin is prepared from the following components in parts by mass: 180 to 280 parts of unsaturated binary acid, 200 to 300 parts of dihydric alcohol, 300 to 500 parts of styrene, 0.05 to 0.15 part of polymerization inhibitor, 0.3 to 2 parts of catalyst, 12 to 20 parts of modified filler, 4 to 12 parts of nano titanium dioxide, 2 to 5 parts of additive and 300 to 500 parts of water. Aiming at the problems of toughness and durability of the existing unsaturated polyester resin, the invention discloses a new scheme: three unsaturated diacids and dihydric alcohol are used as main synthesis raw materials to synthesize an unsaturated polyester resin main body, and compared with a single unsaturated polyester component, the unsaturated polyester resin main body has the advantages that the performance is obviously improved, the steric hindrance relationship among molecules and group coordination are realized, and the toughness and durability of the unsaturated polyester resin are improved. The stability and durability of the air guide sleeve can be obviously improved; and three fibers are adopted for filling, so that the reinforcing effect is achieved, the toughening effect is improved, and the overall mechanical property and impact strength are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyester resins, and in particular relates to a bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing. Background Art

[0002] The deflector is an air deflector installed on the top of the cab of a car or a tractor. Its main function is to effectively reduce the air resistance and fuel consumption when the vehicle is driving at high speed. The current deflector has replaced the original main wing and two-side combination type with an integral type. The front and side surfaces are pressed with exquisitely designed reinforcing ribs or a skeleton is added on the back to withstand the wind force when the car is driving. Usually, when the deflector is produced, a hot pressing molding device is used to hot press the glass reinforced polyester fiber to produce the deflector. The existing deflector molded composite materials are still insufficient in toughness, durability, and environmental protection. In particular, the new energy vehicle industry has higher requirements for the shell material. Car companies pay special attention to the pressure resistance and environmental protection of the material. The main raw material of the deflector material can be selected from unsaturated polyester resin, which has a lot of room for optimization and improvement.

[0003] Unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by polycondensation of unsaturated dibasic acids and diols. As global environmental issues become increasingly prominent, people are paying more and more attention to the improvement of environmental awareness. Environmentally friendly unsaturated polyester resin has important significance and value in promoting the application of new energy vehicle fairing materials, the development of environmental protection industry, promoting sustainable development, improving the living environment and maintaining ecological balance. Summary of the invention

[0004] In view of the current problems of toughness, durability and environmental protection of unsaturated polyester resins, the present invention aims to provide a bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings.

[0005] A bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing, comprising the following components by weight:

[0006] 180-280 parts of unsaturated dibasic acid, 200-300 parts of diol, 300-500 parts of styrene, 0.05-0.15 parts of inhibitor, 0.3-2 parts of catalyst, 12-20 parts of modified filler, 4-12 parts of nano titanium dioxide, 2-5 parts of additives, and 300-500 parts of water.

[0007] Furthermore, the unsaturated dibasic acid is a combination of itaconic acid, fumaric acid and phthalic anhydride in a mass ratio of 1:2-5:10-15.

[0008] Furthermore, the diol is selected from a combination of 1,2-propylene glycol, neopentyl glycol, and polytetramethylene ether glycol in a mass ratio of 3 to 7:1:8.

[0009] Furthermore, the polymerization inhibitor is any one of o-methylhydroquinone and p-tert-butylhydroquinone.

[0010] Furthermore, the catalyst is any one of tetrabutyl titanate, tetraisopropyl titanate, and monobutyl tin oxide.

[0011] Furthermore, the modified filler is a combination of glass fiber, flax fiber and bamboo charcoal fiber in a mass ratio of 3 to 7:2:1.

[0012] Furthermore, the particle size of the glass fiber is 0.4-1 micron, the particle size of the flax fiber is 0.5-1 micron, and the particle size of the bamboo charcoal fiber is 0.02-0.08 micron.

[0013] Furthermore, the additive is: epoxy castor oil and carbon nanotubes are mixed at a mass ratio of 4 to 8:1; the particle size of the carbon nanotubes is 0.1 to 0.5 microns.

[0014] Furthermore, the preparation of the unsaturated polyester resin comprises the following steps:

[0015] (1) Take 180-280 parts of unsaturated dibasic acid, 200-300 parts of diol, 300-500 parts of styrene, 0.05-0.15 parts of polymerization inhibitor, 0.3-2 parts of catalyst, 12-20 parts of modified filler, 4-12 parts of nano titanium dioxide, 2-5 parts of additives, and 300-500 parts of water by mass;

[0016] (2) Under nitrogen protection, unsaturated dibasic acid and water are mixed and preheated at 80-110°C; diol is added, the temperature is raised to 120-130°C for reflux reaction, inhibitor and catalyst are added, the temperature is slowly raised to 195-205°C, the temperature is kept, and additives are added; vacuum reaction is performed to obtain polyester; the polyester is cooled to 140-160°C and the temperature is kept; styrene is added, the temperature is cooled to 60-70°C, modified fillers and nano titanium dioxide are added, and the mixture is mixed and stirred to obtain a bio-based unsaturated polyester resin that can be used for new energy vehicle fairing molding composite materials.

[0017] Furthermore, in the step (2), the treatment time of the reflux reaction process of heating to 120-130° C. is 2-3 hours, until the acid value of the reactant reaches between 30 and 35 mgKOH / g.

[0018] Compared with the prior art, the advantages of the present invention are:

[0019] The invention adopts three unsaturated dibasic acids and diols as main synthetic raw materials to synthesize an unsaturated polyester resin main body, which has significantly improved performance compared with a single unsaturated polyester component. The steric hindrance relationship and group coordination between molecules can significantly improve the stability and durability when applied to the deflector cover of new energy vehicles; the combination of epoxidized castor oil and carbon nanotubes in the additive can comprehensively improve the mechanical effect of the unsaturated polyester system; the epoxy group and hydroxyl group carried by the epoxidized castor oil can be combined with the unsaturated polyester to obtain a more stable structure resistant to external stress, and the bonding force between the components of the system can be improved; in addition, the oxidized castor oil can also undergo self-crosslinking to improve the interface bonding ability between the blends and form a stable phase morphology; the added carbon nanotubes can also provide a synergistic toughening effect; glass fiber, flax fiber and bamboo charcoal fiber are used as modified fillers, and the three fiber components have good dispersibility and can play a reinforcing role, which is beneficial to improving the toughening effect and improving the overall mechanical properties and impact resistance. DETAILED DESCRIPTION

[0020] The following is a specific embodiment of a bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing of the present invention. It is necessary to point out that the following examples are only used to explain the present invention in more detail, rather than to narrow the scope of protection of the present invention. After reading the present invention, improvements and adjustments made by professionals in this technical field without departing from the concept of the present invention are within the scope of protection claimed by the present invention.

[0021] A bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing, comprising the following components by weight:

[0022] 180-280 parts of unsaturated dibasic acid, 200-300 parts of diol, 300-500 parts of styrene, 0.05-0.15 parts of inhibitor, 0.3-2 parts of catalyst, 12-20 parts of modified filler, 4-12 parts of nano titanium dioxide, 2-5 parts of additives, and 300-500 parts of water.

[0023] The unsaturated dibasic acid is selected from itaconic acid, fumaric acid and phthalic anhydride in a mass ratio of 1:2-5:10-15.

[0024] The diol is a combination of 1,2-propylene glycol, neopentyl glycol and polytetramethylene ether glycol in a mass ratio of 3 to 7:1:8.

[0025] The polymerization inhibitor is selected from any one of o-methyl hydroquinone and p-tert-butyl hydroquinone.

[0026] The catalyst is any one of tetrabutyl titanate, tetraisopropyl titanate and monobutyl tin oxide.

[0027] Modified filler: a combination of glass fiber, flax fiber and bamboo charcoal fiber in a mass ratio of 3 to 7:2:1.

[0028] The particle size of glass fiber is 0.4-1 micron, the particle size of flax fiber is 0.5-1 micron, and the particle size of bamboo charcoal fiber is 0.02-0.08 micron.

[0029] Additives: epoxy castor oil and carbon nanotubes are mixed in a mass ratio of 4 to 8:1; the particle size of the carbon nanotubes is 0.1 to 0.5 microns.

[0030] A method for preparing a bio-based unsaturated polyester resin for use in a molded composite material for a new energy vehicle fairing comprises the following steps:

[0031] (1) Take 180-280 parts of unsaturated dibasic acid, 200-300 parts of diol, 300-500 parts of styrene, 0.05-0.15 parts of polymerization inhibitor, 0.3-2 parts of catalyst, 12-20 parts of modified filler, 4-12 parts of nano titanium dioxide, 2-5 parts of additives, and 300-500 parts of water by mass;

[0032] (2) Under nitrogen protection, unsaturated dibasic acid and water are mixed and preheated at 80-110°C for 30-50 min; diol is added, the temperature is raised to 120-130°C, reflux reaction is carried out for 2-3 h until the acid value of the reactant reaches 30-35 mgKOH / g, inhibitor and catalyst are added, the temperature is slowly raised to 195-205°C, the temperature is kept for 2-3 h, and additives are added; vacuum reaction is carried out for 1-2 h to obtain polyester; the polyester is cooled to 140-160°C and the temperature is kept for 1-2 h; styrene is added, the temperature is lowered to 60-70°C, modified filler and nano titanium dioxide are added, and the mixture is mixed and stirred for 1-2 h to obtain a bio-based unsaturated polyester resin that can be used for molded composite materials of new energy vehicle fairings.

[0033] Example 1

[0034] A bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing, comprising the following components by weight:

[0035] 180 parts of unsaturated dibasic acid, 200 parts of diol, 300 parts of styrene, 0.05 parts of inhibitor, 0.3 parts of catalyst, 12 parts of modified filler, 4 parts of nano titanium dioxide, 2 parts of additives, and 300-500 parts of water.

[0036] The unsaturated dibasic acid is a combination of itaconic acid, fumaric acid and phthalic anhydride in a mass ratio of 1:3:12.

[0037] The diol is a combination of 1,2-propylene glycol, neopentyl glycol and polytetramethylene ether glycol in a mass ratio of 3:1:8.

[0038] The inhibitor is o-methylhydroquinone.

[0039] Tetrabutyl titanate was selected as the catalyst.

[0040] Modified filler: a combination of glass fiber, flax fiber and bamboo charcoal fiber in a mass ratio of 3:2:1.

[0041] The particle size of glass fiber is 0.4 microns, the particle size of flax fiber is 0.5 microns, and the particle size of bamboo charcoal fiber is 0.02 microns.

[0042] Additives: Mix epoxy castor oil and carbon nanotubes in a mass ratio of 4:1; the particle size of the carbon nanotubes is 0.1 micron.

[0043] A method for preparing a bio-based unsaturated polyester resin for use in a molded composite material for a new energy vehicle fairing comprises the following steps:

[0044] (1) Take 180 parts of unsaturated dibasic acid, 200 parts of diol, 300 parts of styrene, 0.05 parts of polymerization inhibitor, 0.3 parts of catalyst, 12 parts of modified filler, 4 parts of nano titanium dioxide, 2 parts of additives, and 300-500 parts of water by mass;

[0045] (2) Under nitrogen protection, unsaturated dibasic acid and water are mixed and preheated at 80°C for 30 min; diol is added, the temperature is raised to 120°C and refluxed for 2 h until the acid value of the reactant reaches 30 mgKOH / g, inhibitor and catalyst are added, the temperature is slowly raised to 195°C and kept warm for 2 h, and additives are added; vacuum reaction is carried out for 1 h to obtain polyester; the polyester is cooled to 140°C and kept warm for 1 h; styrene is added, the temperature is lowered to 60°C, modified fillers and nano titanium dioxide are added, and the mixture is mixed and stirred for 1 h to obtain a bio-based unsaturated polyester resin that can be used in new energy vehicle fairing molding composite materials.

[0046] Example 2

[0047] A bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing, comprising the following components by weight:

[0048] 250 parts of unsaturated dibasic acid, 250 parts of diol, 400 parts of styrene, 0.1 parts of inhibitor, 1 part of catalyst, 16 parts of modified filler, 10 nano titanium dioxide, 3 parts of additives, and 400 parts of water.

[0049] The unsaturated dibasic acid is a combination of itaconic acid, fumaric acid and phthalic anhydride in a mass ratio of 1:4:12.

[0050] The diol is a combination of 1,2-propylene glycol, neopentyl glycol and polytetramethylene ether glycol in a mass ratio of 5:1:8.

[0051] The polymerization inhibitor is tert-butylhydroquinone.

[0052] Tetrabutyl titanate was selected as the catalyst.

[0053] Modified filler: a combination of glass fiber, flax fiber and bamboo charcoal fiber in a mass ratio of 5:2:1.

[0054] The particle size of glass fiber is 0.7 micron, the particle size of flax fiber is 0.7 micron, and the particle size of bamboo charcoal fiber is 0.06 micron.

[0055] Additives: Mix epoxy castor oil and carbon nanotubes in a mass ratio of 5:1; the particle size of the carbon nanotubes is 0.3 microns.

[0056] A method for preparing a bio-based unsaturated polyester resin for use in a molded composite material for a new energy vehicle fairing comprises the following steps:

[0057] (1) Take 250 parts of unsaturated dibasic acid, 250 parts of diol, 400 parts of styrene, 0.1 parts of polymerization inhibitor, 1 part of catalyst, 16 parts of modified filler, 10 nano titanium dioxide, 3 parts of additives, and 400 parts of water by mass;

[0058] (2) Under nitrogen protection, unsaturated dibasic acid and water are mixed and preheated at 90°C for 40 min; diol is added, the temperature is raised to 125°C and refluxed for 3 h until the acid value of the reactant reaches 35 mgKOH / g, inhibitor and catalyst are added, the temperature is slowly raised to 205°C and kept warm for 3 h, and additives are added; vacuum reaction is carried out for 2 h to obtain polyester; the polyester is cooled to 140°C and kept warm for h; styrene is added, the temperature is lowered to 70°C, modified fillers and nano titanium dioxide are added, and the mixture is mixed and stirred for 2 h to obtain a bio-based unsaturated polyester resin that can be used for molding composite materials of new energy vehicle fairings.

[0059] Example 3

[0060] A bio-based unsaturated polyester resin used in a molded composite material for a new energy vehicle fairing, comprising the following components by weight:

[0061] 280 parts of unsaturated dibasic acid, 300 parts of diol, 500 parts of styrene, 0.15 parts of inhibitor, 2 parts of catalyst, 20 parts of modified filler, 12 parts of nano titanium dioxide, 5 parts of additives, and 500 parts of water.

[0062] The unsaturated dibasic acid is a combination of itaconic acid, fumaric acid and phthalic anhydride in a mass ratio of 1:5:15.

[0063] The diol is a combination of 1,2-propylene glycol, neopentyl glycol and polytetramethylene ether glycol in a mass ratio of 7:1:8.

[0064] The inhibitor is o-methylhydroquinone.

[0065] Tetrabutyl titanate was selected as the catalyst.

[0066] Modified filler: a combination of glass fiber, flax fiber and bamboo charcoal fiber in a mass ratio of 7:2:1.

[0067] The particle size of glass fiber is 1 micron, the particle size of flax fiber is 1 micron, and the particle size of bamboo charcoal fiber is 0.08 micron.

[0068] Additives: Mix epoxy castor oil and carbon nanotubes in a mass ratio of 8:1; the particle size of the carbon nanotubes is 0.5 microns.

[0069] A method for preparing a bio-based unsaturated polyester resin for use in a molded composite material for a new energy vehicle fairing comprises the following steps:

[0070] (1) Take 280 parts of unsaturated dibasic acid, 300 parts of diol, 500 parts of styrene, 0.15 parts of polymerization inhibitor, 2 parts of catalyst, 20 parts of modified filler, 12 parts of nano titanium dioxide, 5 parts of additives and 500 parts of water by mass.

[0071] (2) Under nitrogen protection, unsaturated dibasic acid and water are mixed and preheated at 100°C for 50 min; diol is added, the temperature is raised to 120-130°C and refluxed for 3 h until the acid value of the reactant reaches 35 mgKOH / g, inhibitor and catalyst are added, the temperature is slowly raised to 205°C and kept warm for 3 h, and additives are added; vacuum reaction is carried out for 2 h to obtain polyester; the polyester is cooled to 160°C and kept warm for 2 h; styrene is added, the temperature is cooled to 70°C, modified fillers and nano titanium dioxide are added, and the mixture is mixed and stirred for 2 h to obtain a bio-based unsaturated polyester resin that can be used in new energy vehicle fairing molding composite materials.

[0072] Comparative Example 1: It is basically the same as Example 2, except that the modified filler is missing.

[0073] Comparative Example 2: It is basically the same as Example 2, except that the additive is missing.

[0074] Comparative Example 3: Commercially available bio-based unsaturated polyester resin in Nanjing.

[0075] The unsaturated resins obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were uniformly tested for tensile strength, elongation at break and notched impact strength, wherein the tensile strength and elongation at break were measured according to GB / T1040.2-2006 standard; the notched impact strength was measured according to GB / T1043.1-2008 standard. The test results are shown in Table 1 below:

[0076] Table 1

[0077]

[0078]

[0079] As can be seen from Table 1, the products obtained in Examples 1 to 3 are subjected to tensile strength, elongation at break and notched impact strength tests, and have obvious advantages over the results obtained in Comparative Example 3. Comparative Example 1 lacks modified fillers, resulting in a significant decrease in test performance; Comparative Example 2 lacks additives, resulting in a certain degree of decrease in test performance.

[0080] Note: The above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention; therefore, although this specification has described the present invention in detail with reference to the above embodiments, a person skilled in the art should understand that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements thereof that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A bio-based unsaturated polyester resin used in molded composite materials for new energy vehicle fairings, characterized in that: The components are as follows by mass: 180-280 parts of unsaturated dibasic acid, 200-300 parts of diol, 300-500 parts of styrene, 0.05-0.15 parts of inhibitor, 0.3-2 parts of catalyst, 12-20 parts of modified filler, 4-12 parts of nano titanium dioxide, 2-5 parts of additives, and 300-500 parts of water.

2. The bio-based unsaturated polyester resin used for molded composite materials of new energy vehicle fairings according to claim 1, characterized in that: The unsaturated dibasic acid is a combination of itaconic acid, fumaric acid and phthalic anhydride in a mass ratio of 1:2-5:10-15.

3. The bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 1, characterized in that: The diol is selected from a combination of 1,2-propylene glycol, neopentyl glycol and polytetramethylene ether glycol in a mass ratio of 3 to 7:1:

8.

4. The bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 1, characterized in that: The polymerization inhibitor is any one of o-methylhydroquinone and p-tert-butylhydroquinone.

5. The bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 1, characterized in that: The catalyst is any one of tetrabutyl titanate, tetraisopropyl titanate and monobutyl tin oxide.

6. The method for preparing the bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 1, characterized in that: The modified filler is a combination of glass fiber, flax fiber and bamboo charcoal fiber in a mass ratio of 3-7:2:

1.

7. The method for preparing the bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 6, characterized in that: The particle size of the glass fiber is 0.4-1 micron, the particle size of the flax fiber is 0.5-1 micron, and the particle size of the bamboo charcoal fiber is 0.02-0.08 micron.

8. The method for preparing the bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 1, characterized in that: The additive is: epoxy castor oil and carbon nanotubes are mixed in a mass ratio of 4 to 8:1; the particle size of the carbon nanotubes is 0.1 to 0.5 microns.

9. The bio-based unsaturated polyester resin for use in molded composite materials for new energy vehicle fairings according to claim 1, characterized in that: The preparation of the unsaturated polyester resin comprises the following steps: (1) Take 180-280 parts of unsaturated dibasic acid, 200-300 parts of diol, 300-500 parts of styrene, 0.05-0.15 parts of polymerization inhibitor, 0.3-2 parts of catalyst, 12-20 parts of modified filler, 4-12 parts of nano titanium dioxide, 2-5 parts of additives, and 300-500 parts of water by mass; (2) Under nitrogen protection, unsaturated dibasic acid and water are mixed and preheated at 80-110°C; diol is added, the temperature is raised to 120-130°C for reflux reaction, inhibitor and catalyst are added, the temperature is slowly raised to 195-205°C, the temperature is kept, and additives are added; vacuum reaction is performed to obtain polyester; the polyester is cooled to 140-160°C and the temperature is kept; styrene is added, the temperature is cooled to 60-70°C, modified fillers and nano titanium dioxide are added, and the mixture is mixed and stirred to obtain a bio-based unsaturated polyester resin that can be used for new energy vehicle fairing molding composite materials.

10. The bio-based unsaturated polyester resin used for molded composite materials of new energy vehicle fairings according to claim 9, characterized in that: In the step (2), the temperature is raised to 120-130° C. and the reflux reaction is carried out for 2-3 hours until the acid value of the reactant reaches between 30 and 35 mgKOH / g.