Mute wear-resistant thermoplastic elastomer material and preparation method thereof
By using materials such as hydrogenated styrene-butadiene block copolymers in thermoplastic elastomers, combinations of alumina microsphere powders and modified boron nitride powders, the problems of insufficient hardness and high noise of thermoplastic elastomers are solved. , achieving better wear resistance and silent effect.
Patent Information
- Application Number
- CN202411431954.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In sweeping robots, thermoplastic elastomers cannot meet the wear resistance requirements due to insufficient hardness and rough surface, resulting in greater noise during friction.
Using hydrogenated styrene-butadiene block copolymer, filler oil, zinc stearate, polypropylene, polystyrene, calcium powder, antioxidants, thermoplastic polyurethane elastomers, wear-resistant modifiers and lubricating modifiers The combination of alumina microsphere powder and modified boron nitride powder enhances wear resistance, and reduces the friction coefficient through lubricant microcapsules to achieve a silent effect.
It improves the wear resistance and silent effect of the thermoplastic elastomer, reduces the noise decibels during friction, and enhances the hardness and lubricity of the material.
Smart Images

Figure BDA0005083903630000071 
Figure BDA0005083903630000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of thermoplastic elastomers, and more specifically, to a silent and wear-resistant thermoplastic elastomer material and a preparation method thereof. Background Art
[0002] TPE, or thermoplastic elastomer, is a type of thermoplastic soft rubber that has rubber elasticity and can be directly processed and molded without vulcanization. Its characteristics include good anti-aging, ozone resistance and UV resistance, as well as excellent air tightness, oil resistance, solvent resistance and electrical properties. In addition, TPE is also environmentally friendly, non-toxic and safe, with excellent colorability, weather resistance, fatigue resistance and temperature resistance, excellent processing performance, no need for vulcanization, can be recycled to reduce costs, and can be secondary injection molded or molded alone. Therefore, TPE has been widely used in medical equipment, household appliances, transportation, wires and cables, baby bottles and nipples, high-end sports equipment and other fields.
[0003] When thermoplastic elastomers are used in sweeping robots, they often slide and rub against tiles, glass, etc. during use. The hardness is generally required to be 40-55A. At this hardness, the wear resistance of the thermoplastic elastomer cannot meet the requirements. In addition, since the surface of the thermoplastic elastomer is relatively rough and uneven, the friction coefficient of the surface of the thermoplastic elastomer is relatively large. When it rubs against other objects, it will generate a lot of noise. Summary of the invention
[0004] In order to improve the wear resistance and quiet effect of thermoplastic elastomer materials, the present application provides a quiet and wear-resistant thermoplastic elastomer material and a preparation method thereof.
[0005] In the first aspect, the present application provides a silent and wear-resistant thermoplastic elastomer material, adopting the following technical scheme: a silent and wear-resistant thermoplastic elastomer material, comprising the following raw materials in parts by weight: 40-60 parts of hydrogenated styrene-butadiene block copolymer, 20-35 parts of filler oil, 6-8 parts of zinc stearate, 5-10 parts of polypropylene, 2-3 parts of polystyrene, 1-2 parts of calcium powder, 0.5-0.8 parts of antioxidant, 10-12 parts of thermoplastic polyurethane elastomer, 1-3 parts of wear-resistant modifier and 1-3 parts of lubrication modifier.
[0006] By adopting the above technical scheme, the hydrogenated styrene-butadiene block copolymer has good elasticity and high temperature resistance, the filler oil can effectively adjust the fluidity of the raw material in the molten state and improve its processing performance, zinc stearate as an internal lubricant can reduce the friction between molecules in the molten state of macromolecules, thereby improving the processing performance of TPE, the addition of polypropylene and polystyrene can improve the strength and wear resistance of thermoplastic elastomers, calcium powder used as a filler can improve the wear resistance of thermoplastic elastomers, antioxidants can improve the anti-aging properties of thermoplastic elastomers, thermoplastic polyurethane elastomers can improve the toughness and wear resistance of thermoplastic elastomers, the addition of wear-resistant modifiers can further improve the wear resistance of thermoplastic elastomers, and lubricating modifiers can improve the surface properties of thermoplastic elastomers, reduce the friction coefficient, and reduce the noise decibels emitted when the thermoplastic elastomer rubs against other objects, thereby achieving a silent effect.
[0007] Preferably, the wear-resistant modifier comprises alumina microsphere powder and modified boron nitride powder in a mass ratio of (1.5-1.8):(3.1-3.4).
[0008] By adopting the above technical scheme, both alumina microsphere powder and modified boron nitride powder have high hardness and good high temperature resistance. The microscopic morphology of modified boron nitride powder is flaky, while the microscopic morphology of alumina microsphere powder is spherical. The alumina microsphere powder and modified boron nitride powder are used in combination to enhance the wear resistance and strength of thermoplastic elastomers. At the same time, the flaky structure of the modified boron nitride powder can provide lubricity for the thermoplastic elastomer and improve the quietness effect of the thermoplastic elastomer.
[0009] Preferably, the preparation method of the modified boron nitride powder comprises the following steps: adding boron nitride to isopropanol to obtain a boron nitride isopropanol solution, ultrasonically shaking for 24 hours, centrifuging at 4000-4200r / min for 23-24 hours, taking the upper suspension, centrifuging at 7800-8000r / min for 10-15 minutes, taking the supernatant and air-drying to obtain boron nitride nanosheets, adding the boron nitride nanosheets to water, ultrasonically dispersing them uniformly, adjusting the pH to 8-8.2, adding tetraethyl orthosilicate, hydrolyzing for 5-6 hours, aging for 2-2.5 hours, adding a silane coupling agent and stirring for 3-3.5 hours, filtering and washing to obtain modified boron nitride powder.
[0010] By adopting the above technical scheme, after ultrasonic stratification of boron nitride isopropanol solution, boron nitride can be peeled off to obtain boron nitride nanosheets with fewer layers, and the hydrolysis of tetraethyl orthosilicate can generate silicon dioxide spheres, which are deposited on the surface of the boron nitride nanosheets, further improving the wear resistance of the modified boron nitride powder.
[0011] Preferably, the boron nitride nanosheets are further treated as follows: the boron nitride nanosheets are added to water, ultrasonically dispersed uniformly, dopamine hydrochloride is added, the pH is adjusted to 7.87-8, reacted at 65-70°C for 5-6h, cooled, filtered, and dopamine-modified boron nitride powder is obtained.
[0012] By adopting the above technical solution, dopamine can self-polymerize on the surface of boron nitride nanosheets to form a polydopamine film. The polydopamine film has good adhesion and more active groups, which is beneficial to the deposition of silica spheres on the surface of boron nitride nanosheets.
[0013] Preferably, the lubricating modifier is a lubricant microcapsule, the core of the lubricant microcapsule is oleic acid, and the shell of the lubricant microcapsule is β-cyclodextrin.
[0014] By adopting the above technical solution, the lubricant microcapsules can release oleic acid after being ruptured by force, and the oleic acid can be used as a lubricant, thereby reducing the friction coefficient of the thermoplastic elastomer, thereby reducing the noise generated when the thermoplastic elastomer rubs against other objects and improving the quiet effect of the thermoplastic elastomer.
[0015] Preferably, the method for preparing the lubricant microcapsules comprises the following steps: dissolving β-cyclodextrin in water to obtain a saturated solution, heating to 40-45°C, adding oleic acid dropwise while stirring, reacting for 2-2.5 hours, standing for 24 hours, filtering, washing and drying to obtain the lubricant microcapsules.
[0016] By adopting the above technical solution, β-cyclodextrin can form a shell-like structure with a cavity, which can encapsulate oleic acid. When the lubricant microcapsule is ruptured by force, the oleic acid can be released, thereby reducing the friction coefficient of the thermoplastic elastomer.
[0017] Preferably, the mass ratio of β-cyclodextrin to oleic acid is (5-5.5):(1.2-1.5).
[0018] By adopting the above technical solution, the mass ratio of β-cyclodextrin to oleic acid is controlled, so that the spherical shape of the lubricant microcapsule is better, which is beneficial to improve the encapsulation rate of oleic acid, thereby improving the use effect of the lubricant microcapsule.
[0019] In a second aspect, the present application provides a method for preparing a silent and wear-resistant thermoplastic elastomer material, which adopts the following technical solution: A method for preparing a silent and wear-resistant thermoplastic elastomer material comprises the following steps: uniformly mixing hydrogenated styrene-butadiene block copolymer, filler oil, zinc stearate, polypropylene, polystyrene, calcium powder, antioxidant, thermoplastic polyurethane elastomer, wear-resistant modifier and lubricating modifier, melt blending at 80-120°C to obtain a mixture, and extruding and granulating the mixture at 180-240°C to obtain a finished product.
[0020] By adopting the above technical scheme, the thermoplastic elastomer prepared using this raw material has good elasticity, wear resistance and hardness. When the thermoplastic elastomer is in use, it has good lubricity, generates less noise decibels during friction, and has good quiet effect.
[0021] In summary, this application has the following beneficial effects: 1. Since the present application adopts alumina microsphere powder and modified boron nitride powder as wear-resistant modifiers, both alumina microsphere powder and modified boron nitride powder have high hardness and good high temperature resistance. The microscopic morphology of modified boron nitride powder is flaky, while the microscopic morphology of alumina microsphere powder is spherical. The alumina microsphere powder and modified boron nitride powder are used in combination with each other to enhance the wear resistance and strength of thermoplastic elastomers. At the same time, the flaky structure of modified boron nitride powder can provide lubricity for thermoplastic elastomers and improve the quietness effect of thermoplastic elastomers.
[0022] 2. In the present application, lubricant microcapsules are preferably used as lubricating modifiers. The lubricant microcapsules can release oleic acid after being ruptured by force. Oleic acid can be used as a lubricant, thereby reducing the friction coefficient of the thermoplastic elastomer, thereby reducing the noise generated when the thermoplastic elastomer rubs against other objects and improving the quiet effect of the thermoplastic elastomer. DETAILED DESCRIPTION
[0023] The present application is further described in detail below with reference to the embodiments.
[0024] Preparation Example 1-6 of Modified Boron Nitride Powder Preparation Example 1 Boron nitride was added to isopropanol to obtain a 2.8 g / L boron nitride isopropanol solution. After ultrasonic vibration for 24 hours, the solution was centrifuged at 4000 r / min for 24 hours, the upper suspension was taken, and the solution was centrifuged at 7800 r / min for 15 minutes. The supernatant was air-dried to obtain boron nitride nanosheets. 3 g of boron nitride nanosheets were added to 320 mL of water and ultrasonically dispersed uniformly. After adjusting the pH to 8 with trishydroxymethylaminomethane, 2 mL of ethyl orthosilicate was added, hydrolyzed for 5 hours, aged for 2 hours, 0.2 g of silane coupling agent KH570 was added, stirred for 3 hours, filtered and washed to obtain modified boron nitride powder.
[0025] Preparation Example 2 Boron nitride was added to isopropanol to obtain a 3 g / L boron nitride isopropanol solution. After ultrasonic vibration for 24 hours, the solution was centrifuged at 4200 r / min for 23 hours, the upper suspension was taken, and the solution was centrifuged at 8000 r / min for 10 minutes. The supernatant was air-dried to obtain boron nitride nanosheets. 3 g of boron nitride nanosheets was added to 350 mL of water, and ultrasonic dispersion was performed uniformly. After adjusting the pH to 8.2 with trishydroxymethylaminomethane, 3 mL of ethyl orthosilicate was added, and the solution was hydrolyzed for 6 hours and aged for 2.5 hours. After adding 0.3 g of silane coupling agent KH570 and stirring for 3.5 hours, the solution was filtered and washed to obtain modified boron nitride powder.
[0026] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that the pH is adjusted to 6 in Preparation Example 3.
[0027] Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 1 is that in Preparation Example 4, the pH is adjusted to 10.
[0028] Preparation Example 5 The difference between Preparation Example 5 and Preparation Example 1 is that the boron nitride nanosheets are further treated as follows: 2.8 g of boron nitride nanosheets are added to 350 mL of water, and after ultrasonic dispersion, 0.45 g of dopamine hydrochloride is added, the pH is adjusted to 7.87 with tris(hydroxymethyl)aminomethane, the reaction is carried out at 65°C for 6 hours, the temperature is lowered, and the boron nitride powder modified with dopamine is obtained.
[0029] Preparation Example 6 The difference between Preparation Example 6 and Preparation Example 1 is that the boron nitride nanosheets are further treated as follows: 3 g of boron nitride nanosheets are added to 400 mL of water, and after ultrasonic dispersion, 0.5 g of dopamine hydrochloride is added, the pH is adjusted to 8 with tris(hydroxymethyl)aminomethane, the reaction is carried out at 70°C for 5 h, the temperature is lowered, and the boron nitride powder modified with dopamine is obtained.
[0030] Preparation Examples 7-10 of Lubricant Microcapsules Preparation Example 7 The preparation method of lubricant microcapsules comprises the following steps: dissolving beta-cyclodextrin in water to obtain a saturated solution, heating to 45°C, adding oleic acid dropwise while stirring, reacting for 2 hours, standing for 24 hours, filtering, washing and drying to obtain lubricant microcapsules, wherein the mass ratio of beta-cyclodextrin to oleic acid is 5:1.2.
[0031] Preparation Example 8 The preparation method of lubricant microcapsules comprises the following steps: dissolving β-cyclodextrin in water to obtain a saturated solution, heating to 40°C, adding oleic acid dropwise while stirring, reacting for 2.5 hours, standing for 24 hours, filtering, washing and drying to obtain lubricant microcapsules, wherein the mass ratio of β-cyclodextrin to oleic acid is 5.5:1.5.
[0032] Preparation Example 9 The difference between Preparation Example 9 and Preparation Example 7 is that in Preparation Example 9, the mass ratio of β-cyclodextrin to oleic acid is 5:0.5.
[0033] Preparation Example 10 The difference between Preparation Example 10 and Preparation Example 7 is that in Preparation Example 10, the mass ratio of β-cyclodextrin to oleic acid is 5:3. Example
[0034] Example 1 A silent and wear-resistant thermoplastic elastomer material, characterized in that it comprises the following raw materials in parts by weight: 40kg hydrogenated styrene-butadiene block copolymer, 20kg filling oil, 6kg zinc stearate, 5kg polypropylene, 2kg polystyrene, 1kg calcium powder, 0.5kg antioxidant, 10kg thermoplastic polyurethane elastomer, 1kg wear-resistant modifier and 1kg lubricating modifier, wherein the hydrogenated styrene-butadiene block copolymer is purchased from Dongguan Longsheng Engineering Plastics Co., Ltd., model 503T, the filling oil is paraffin oil, purchased from Beijing Zeping Technology Co., Ltd., zinc stearate is purchased from Gaomi Xinwei Additive Co., Ltd., and polypropylene is purchased from Yanshan Petrochemical Company, model 134 0, polystyrene was purchased from Qingdao Zhongxin Huamei Plastic Co., Ltd., model PG-383M, calcium powder was purchased from Qingyuan Gaofeng Powder Co., Ltd., antioxidant was purchased from Nanjing Milan Chemical Co., Ltd., model antioxidant 5057, thermoplastic polyurethane elastomer was purchased from Qingdao Zhuoli Rubber and Plastic Material Co., Ltd., model UT6-85AU10, wear-resistant modifier includes alumina microsphere powder and modified boron nitride powder with a mass ratio of 1.5:3.1, alumina microsphere powder was purchased from Lianyungang Rongbai New Materials Co., Ltd., model AL203, modified boron nitride powder is modified boron nitride powder prepared in Preparation Example 1, lubricant modifier is lubricant microcapsule, and lubricant microcapsule prepared in Preparation Example 7 is selected.
[0035] The preparation method of the above-mentioned silent and wear-resistant thermoplastic elastomer material comprises the following steps: uniformly mixing hydrogenated styrene-butadiene block copolymer, filler oil, zinc stearate, polypropylene, polystyrene, calcium powder, antioxidant, thermoplastic polyurethane elastomer, wear-resistant modifier and lubricating modifier, melt blending at 120°C to obtain a mixture, and extruding and granulating the mixture at 180°C to obtain a finished product.
[0036] Example 2 A silent and wear-resistant thermoplastic elastomer material, characterized in that it comprises the following raw materials in parts by weight: 60kg hydrogenated styrene-butadiene block copolymer, 35kg filling oil, 8kg zinc stearate, 10kg polypropylene, 3kg polystyrene, 2kg calcium powder, 0.8kg antioxidant, 112kg thermoplastic polyurethane elastomer, 3kg wear-resistant modifier and 3kg lubricating modifier, wherein the hydrogenated styrene-butadiene block copolymer is purchased from Dongguan Longsheng Engineering Plastics Co., Ltd., model 503T, the filling oil is paraffin oil, purchased from Beijing Zeping Technology Co., Ltd., zinc stearate is purchased from Gaomi Xinwei Additive Co., Ltd., polypropylene is purchased from Yanshan Petrochemical Company, model 13 40, polystyrene was purchased from Qingdao Zhongxin Huamei Plastic Co., Ltd., model PG-383M, calcium powder was purchased from Qingyuan Gaofeng Powder Co., Ltd., antioxidant was purchased from Nanjing Milan Chemical Co., Ltd., model antioxidant 5057, thermoplastic polyurethane elastomer was purchased from Qingdao Zhuoli Rubber and Plastic Material Co., Ltd., model UT6-85AU10, wear-resistant modifier included alumina microsphere powder and modified boron nitride powder in a mass ratio of 1.8:3.4, alumina microsphere powder was purchased from Lianyungang Rongbai New Materials Co., Ltd., model AL203, modified boron nitride powder was selected from the modified boron nitride powder prepared in Preparation Example 2, lubricating modifier was lubricant microcapsule, and lubricant microcapsule prepared in Preparation Example 8 was selected.
[0037] The preparation method of the above-mentioned silent and wear-resistant thermoplastic elastomer material comprises the following steps: uniformly mixing hydrogenated styrene-butadiene block copolymer, filler oil, zinc stearate, polypropylene, polystyrene, calcium powder, antioxidant, thermoplastic polyurethane elastomer, wear-resistant modifier and lubricating modifier, melt blending at 80°C to obtain a mixture, and extruding and granulating the mixture at 240°C to obtain a finished product.
[0038] Example 3 The difference between Example 3 and Example 1 is that in Example 3, the wear-resistant modifier includes alumina microsphere powder and modified boron nitride powder in a mass ratio of 1.5:1.5.
[0039] Example 4 The difference between Example 4 and Example 1 is that in Example 4, the wear-resistant modifier includes alumina microsphere powder and modified boron nitride powder in a mass ratio of 1.5:4.
[0040] Example 5 The difference between Example 5 and Example 1 is that in Example 5, the modified boron nitride powder is the modified boron nitride powder prepared in Preparation Example 3.
[0041] Example 6 The difference between Example 6 and Example 1 is that in Example 6, the modified boron nitride powder is the modified boron nitride powder prepared in Preparation Example 4.
[0042] Example 7 The difference between Example 7 and Example 1 is that in Example 7, the modified boron nitride powder is the modified boron nitride powder prepared in Preparation Example 5.
[0043] Example 8 The difference between Example 8 and Example 1 is that in Example 8, the modified boron nitride powder is the modified boron nitride powder prepared in Preparation Example 6.
[0044] Example 9 The difference between Example 9 and Example 1 is that in Example 9, the lubricant microcapsules are the lubricant microcapsules prepared in Preparation Example 9.
[0045] Example 10 The difference between Example 10 and Example 1 is that in Example 10, the lubricant microcapsules are the lubricant microcapsules prepared in Preparation Example 10.
[0046] Embodiment 11 The difference between Example 11 and Example 1 is that in Example 11, an equal amount of alumina microsphere powder is used instead of the wear-resistant modifier.
[0047] Example 12 The difference between Example 12 and Example 1 is that in Example 12, an equal amount of modified boron nitride powder is used instead of the wear-resistant modifier, and the modified boron nitride powder is the modified boron nitride powder prepared in Preparation Example 1.
[0048] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that no wear-resistant modifier is added in Comparative Example 1.
[0049] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that no lubricity modifier is added in Comparative Example 2.
[0050] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that in Comparative Example 3, the following raw materials are included in parts by weight: 50 kg of hydrogenated styrene-butadiene block copolymer, 30 kg of filler oil, 3 kg of zinc stearate, 2 kg of polypropylene, 5 kg of polystyrene, 3 kg of calcium powder, 0.5 kg of antioxidant, 5 kg of thermoplastic polyurethane elastomer, 0.5 kg of wear-resistant modifier and 0.9 kg of lubricity modifier.
[0051] Test methods According to the raw materials and preparation methods of Examples 1-12 and Comparative Examples 1-3, silent and wear-resistant thermoplastic elastomer samples were prepared, and the samples were placed on a friction and wear testing machine for wear testing. The test method was based on GB / T 9867-2008 Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrader method), and the results were recorded in Table 1. At the same time, a decibel meter was used to measure the sound decibels at the test site, and the results were recorded in Table 1.
[0052] Table 1 Wear resistance and noise reduction effect of thermoplastic elastomers According to Table 1, Examples 1-2 and Comparative Examples 1-3, it can be known that the wear resistance of the thermoplastic elastomer material prepared in Examples 1-2 is better than that in Comparative Examples 1-3, and the thermoplastic elastomer material prepared in Examples 1-2 has less noise during the friction process. Compared with Examples 1-2, Comparative Example 1 does not add a wear-resistant modifier in Comparative Example 1, and the wear-resistant modifier is formed by a composite of alumina microsphere powder and modified boron nitride powder. Both the alumina microsphere powder and the modified boron nitride powder have good hardness and high temperature resistance. The microscopic morphology of the alumina microsphere powder is spherical, while the microscopic morphology of the modified boron nitride powder is flaky. The two have different microscopic morphologies, which can improve the wear resistance of the thermoplastic elastomer from different aspects, thereby improving the wear resistance of the thermoplastic elastomer. At the same time, the flaky structure of the modified boron nitride powder can provide lubricity for the thermoplastic elastomer, thereby improving the mute effect of the thermoplastic elastomer and reducing the noise when it is rubbed.
[0053] Compared with Examples 1-2, in Comparative Example 2, no lubricity modifier is added. The lubricity modifier is a lubricant microcapsule. The core of the lubricant microcapsule is oleic acid. Oleic acid can be used as a lubricant to reduce the friction coefficient of the thermoplastic elastomer, thereby reducing the noise of the thermoplastic elastomer when it is rubbed. The shell of the lubricant microcapsule is β-cyclodextrin. β-cyclodextrin can form a shell structure with a cavity and encapsulate oleic acid therein. When the thermoplastic elastomer is rubbed, the lubricant microcapsule is ruptured by force to release the oleic acid, thereby reducing the friction coefficient of the friction interface, thereby improving the lubricity of the thermoplastic elastomer and reducing the noise volume during friction.
[0054] Compared with Examples 1-2, Comparative Example 3 changes the addition amount of each raw material, which shows that in Examples 1-2, the addition amount of each raw material is moderate, and the wear resistance and lubricity of the prepared thermoplastic elastomer are better. After the change, the synergistic effect between the raw materials will be reduced, thereby reducing the wear resistance and lubricity of the thermoplastic elastomer.
[0055] Compared with Example 1, the wear resistance of the thermoplastic elastomer material prepared in Example 3-4 is inferior to that in Example 1. Example 3-4 adjusts the mass ratio of alumina microsphere powder to modified boron nitride powder in the wear-resistant modifier, indicating that the mass ratio of alumina microsphere powder to modified boron nitride powder has an influence on the effect of the wear-resistant modifier. Alumina microsphere powder and modified boron nitride powder are different in microscopic morphology and can enhance the thermoplastic elastomer from different aspects. There is a synergistic effect between the two. Adjusting the mass ratio between the two can easily make some alumina microsphere powder or modified boron nitride powder unevenly distributed, resulting in agglomeration, or reduce the reinforcement effect on the thermoplastic elastomer, thereby reducing the wear resistance of the thermoplastic elastomer.
[0056] Compared with Example 1, the wear resistance of the thermoplastic elastomer material prepared in Example 5-6 is inferior to that in Example 1, and the thermoplastic elastomer material prepared in Example 5-6 makes more noise when subjected to friction. The modified boron nitride powder used in Example 5-6 is prepared by adjusting the pH of the solution. The pH of the solution will affect the hydrolysis of tetraethyl orthosilicate. When the pH increases, the silicon dioxide formed by the hydrolysis of tetraethyl orthosilicate forms balls separately, which reduces the amount of silicon dioxide deposited on the surface of the boron nitride nanosheets. When the pH decreases, too much silicon dioxide is deposited on the surface of the boron nitride nanosheets, and the morphology is poor, which affects the use effect of the modified boron nitride powder, reduces the wear resistance of the thermoplastic elastomer material, and affects the improvement of the lubricity of the thermoplastic elastomer material by the modified boron nitride powder, resulting in a worse noise reduction effect.
[0057] Compared with Example 1, the wear resistance of the thermoplastic elastomer material prepared in Example 7-8 is better than that in Example 1, and the thermoplastic elastomer material prepared in Example 7-8 makes less noise when subjected to friction. The modified boron nitride powder used in Example 7-8 is treated with dopamine on the boron nitride nanosheets before silicon dioxide is deposited. Dopamine has a good self-polymerization effect and can form a polydopamine layer on the surface of the boron nitride nanosheets, which is beneficial to the deposition of silicon dioxide, thereby improving the morphology of the modified boron nitride powder, improving the effect of the wear-resistant modifier, and at the same time improving the quiet effect of the thermoplastic elastomer material.
[0058] Compared with Example 1, the wear resistance of the thermoplastic elastomer material prepared in Example 9-10 is inferior to that in Example 1, and the thermoplastic elastomer prepared in Example 9-10 makes more noise when subjected to friction. When preparing the lubricant microcapsules used in Example 9-10, the mass ratio of β-cyclodextrin to oleic acid is adjusted. The mass ratio of β-cyclodextrin to oleic acid directly affects the morphology, size and encapsulation rate of the lubricant microcapsules. Too high or too low a mass ratio of the two will result in poor morphology of the lubricant microcapsules and reduced encapsulation rate, thereby affecting the lubricating effect of the lubricant microcapsules and reducing the wear resistance and noise reduction effect of the thermoplastic elastomer.
[0059] Compared with Example 1, the wear resistance of the thermoplastic elastomer material prepared in Examples 11-12 is inferior to that in Example 1, and the thermoplastic elastomer prepared in Examples 11-12 makes more noise when subjected to friction. The wear-resistant modifier in Example 11 only includes alumina microsphere powder, and the wear-resistant modifier in Example 12 only includes modified boron nitride powder. Simply using alumina microsphere powder or modified boron nitride powder as a wear-resistant modifier can improve the wear resistance of the thermoplastic elastomer, but using them separately is not as good as using the two in combination in Example 1, indicating that there is a synergistic effect between alumina microsphere powder and modified boron nitride powder, and the effect of using them together is better.
[0060] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A silent and wear-resistant thermoplastic elastomer material, characterized by: The invention comprises the following raw materials in parts by weight: 40-60 parts of hydrogenated styrene-butadiene block copolymer, 20-35 parts of filler oil, 6-8 parts of zinc stearate, 5-10 parts of polypropylene, 2-3 parts of polystyrene, 1-2 parts of calcium powder, 0.5-0.8 parts of antioxidant, 10-12 parts of thermoplastic polyurethane elastomer, 1-3 parts of wear-resistant modifier and 1-3 parts of lubricity modifier.
2. The silent and wear-resistant thermoplastic elastomer material according to claim 1, characterized in that: The wear-resistant modifier comprises aluminum oxide microsphere powder and modified boron nitride powder in a mass ratio of (1.5-1.8):(3.1-3.4).
3. The silent and wear-resistant thermoplastic elastomer material according to claim 2, characterized in that: The preparation method of the modified boron nitride powder comprises the following steps: adding boron nitride to isopropanol to obtain a boron nitride isopropanol solution, subjecting the solution to ultrasonic vibration for 24 hours, centrifuging at 4000-4200 r / min for 23-24 hours, taking an upper suspension, centrifuging at 7800-8000 r / min for 10-15 minutes, taking a supernatant and air-drying the solution to obtain a boron nitride nanosheet, adding the boron nitride nanosheet into water, uniformly dispersing the solution by ultrasonication, adjusting the pH value to 8-8.2, adding tetraethyl orthosilicate, hydrolyzing the solution for 5-6 hours, aging the solution for 2-2.5 hours, adding a silane coupling agent and stirring the solution for 3-3.5 hours, filtering and washing the solution to obtain the modified boron nitride powder.
4. The silent and wear-resistant thermoplastic elastomer material according to claim 3, characterized in that: The boron nitride nanosheets are further processed as follows: the boron nitride nanosheets are added into water, ultrasonically dispersed uniformly, dopamine hydrochloride is added, the pH is adjusted to 7.87-8, reacted at 65-70° C. for 5-6 hours, cooled, filtered, and dopamine-modified boron nitride powder is obtained.
5. The silent and wear-resistant thermoplastic elastomer material according to claim 1, characterized in that: The lubricating modifier is a lubricant microcapsule, the core of the lubricant microcapsule is oleic acid, and the shell of the lubricant microcapsule is beta-cyclodextrin.
6. The silent and wear-resistant thermoplastic elastomer material according to claim 4, characterized in that: The method for preparing the lubricant microcapsule comprises the following steps: dissolving beta-cyclodextrin in water to obtain a saturated solution, heating to 40-45° C., adding oleic acid dropwise while stirring, reacting for 2-2.5 hours, standing for 24 hours, filtering, washing and drying to obtain the lubricant microcapsule.
7. The silent and wear-resistant thermoplastic elastomer material according to claim 6, characterized in that: The mass ratio of the β-cyclodextrin to oleic acid is (5-5.5):(1.2-1.5).
8. The method for preparing a silent and wear-resistant thermoplastic elastomer material according to any one of claims 1 to 7, characterized in that: The following steps are involved: The hydrogenated styrene-butadiene block copolymer, filler oil, zinc stearate, polypropylene, polystyrene, calcium powder, antioxidant, thermoplastic polyurethane elastomer, wear-resistant modifier and lubricity modifier are uniformly mixed, melt-blended at 80-120° C. to obtain a mixture, and the mixture is extruded and granulated at 180-240° C. to obtain a finished product.
Citation Information
Patent Citations
SBC thermoplastic elastic material and preparation technology thereof
CN105255092A
TPE high-elasticity castor material and preparation method thereof
CN107057263A
Wear-resistant environment-friendly wood grain decorative PP film and preparation method thereof
CN117624694A