Biodegradable composite material based on PHBH and natural plant fibers and preparation
Through the combination of alkali treatment and coupling agent, the interface compatibility between PHBH and bamboo fibers is improved, the mechanical properties and cost problems of composite materials are solved, and high-performance and environmentally friendly biodegradable composite materials are achieved.
Patent Information
- Application Number
- CN202411422361.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
The existing PHBH matrix and natural plant fiber composites have problems such as poor mechanical properties, poor interfacial compatibility and high cost.
Using a combination of alkali treatment and coupling agent, the lignin and other substances on the surface of plant fibers are removed through alkali treatment, and the roughness of the fiber surface is increased. Titanate coupling agents are used to enhance the interface binding force, thereby improving PHBH and bamboo. Interface compatibility of fibers.
It significantly improves the mechanical properties and interface compatibility of composite materials, while reducing production costs and maintaining biodegradability and environmentally friendly properties.
Smart Images

Figure CN119081377A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biodegradable composite materials, and relates to a biodegradable composite material based on poly (3-hydroxybutyric acid-co-3-hydroxyhexanoic acid) PHBH and natural plant fibers; specifically, it relates to a preparation method of a biodegradable plastic containing natural plant fibers and taking poly (3-hydroxybutyric acid-co-3-hydroxyhexanoic acid) (PHBH) as a matrix. Background Art
[0002] With the development of science and technology, industrial production has become increasingly developed. Polymer materials are difficult to degrade in the natural environment, resulting in non-degradable polymer materials mainly relying on landfill or incineration. These treatment methods not only take up a lot of space, but also cause irreversible pollution to the environment, and the impact and harm are becoming increasingly severe. Therefore, people have gradually realized the importance and urgency of protecting the environment, and the research and development and use of environmentally friendly materials such as degradable materials and natural materials have become the focus and hotspot of research.
[0003] Poly(3-hydroxybutyric acid-co-3-hydroxyhexanoic acid) (PHBH) is one of the most widely used biodegradable polymers with good biocompatibility and renewability. Natural plant fibers have the advantages of renewability, biodegradability, low density, excellent mechanical properties, good processing properties, diversity and adjustability in the preparation of degradable composite materials. These characteristics make natural plant fibers an important choice for the preparation of environmentally friendly materials.
[0004] However, previous studies have found that although the cost of some biodegradable materials can be reduced by modifying natural plant fibers, the poor compatibility with PHBH has an adverse effect on the mechanical properties, thermal properties and crystallization properties of the materials. In order to solve the interfacial compatibility problem between PHBH and bamboo fiber powder, the present invention adopts a method combining alkali treatment and coupling agent. Alkali treatment can remove substances such as lignin, hemicellulose, pectin, wax and grease on the surface of plant fibers, thereby increasing the roughness of the fiber surface and increasing the contact area with the PHBH matrix to improve the interfacial bonding ability. Taking titanate coupling agent as an example, when it is used to treat bamboo fibers, -OC3H 7 The group can couple with the hydroxyl groups on the surface of bamboo fiber to reduce the surface polarity. The octanoate group is entangled with the molecular chain of the PHBH matrix during the blending process, enhancing the bonding force between the two phases. The pyrophosphate group can not only enhance the bonding performance, improve the dispersibility and flame retardancy in the composite material, but also decompose into phosphate groups after contacting with free water when blended with bamboo fiber powder, further improving the coupling effect between the coupling agent and the bamboo fiber powder, thereby improving the interface compatibility between the matrix and the filler, and then improving the mechanical properties. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide an environmentally friendly, economical PHBH / bamboo fiber composite material with excellent mechanical properties and excellent interface compatibility, in order to address the defects of existing composite materials prepared from PHBH matrix and natural plant fibers, such as poor mechanical properties, poor interface compatibility and high cost.
[0006] The technical solution of the present invention is: a biodegradable composite material based on poly (3-hydroxybutyric acid-co-3-hydroxyhexanoic acid) PHBH and natural plant fiber according to the present invention, wherein the mass percentage of each component in the composite material is: PHBH matrix: 80% to 85%, bamboo fiber powder: 10% to 15%, and coupling agent: 0 to 5%.
[0007] Furthermore, the mass percentages of the components in the composite material are: PHBH matrix: 85%, bamboo fiber powder: 10%, coupling agent: 5%.
[0008] Furthermore, the bamboo fiber powder is selected from natural plant fiber, which has a yellow powdery solid appearance, is used as a reinforcing filler, and is modified by alkali treatment;
[0009] Furthermore, the present invention also provides a modified additive for improving the interfacial compatibility between the PHBH matrix and the natural plant fiber, namely a coupling agent, which is selected from at least one of an aluminate coupling agent, a titanate coupling agent and an aluminum titanate coupling agent.
[0010] Furthermore, a method for preparing a biodegradable composite material based on PHBH and natural plant fibers comprises the following steps:
[0011] Step (1): treating the bamboo fiber powder with alkali to expose the hydroxyl groups on its surface;
[0012] Step (2): adding a coupling agent to the modified bamboo fiber powder to obtain a blend of the bamboo fiber powder and the coupling agent;
[0013] Step (3): The prepared blend of bamboo fiber powder and coupling agent is mixed with a PHBH matrix in proportion, and processed by a melt blending process to finally prepare a biodegradable composite material based on PHBH and natural plant fibers.
[0014] Furthermore, in step (1), the concentration of alkali solution required for alkali treatment of the bamboo fiber powder is 1%, 3%, 5%, 7% or 9%.
[0015] Furthermore, in step (1), after the bamboo fiber powder is subjected to alkali treatment, the weighed alkali-pretreated bamboo fiber powder and the prepared PHBH flake solid are placed in an oven, the temperature is set to 60° C., and dried for 48 hours to remove the remaining moisture in the PHBH flake solid.
[0016] Furthermore, in step (2), the coupling agent is added to the modified bamboo fiber powder in proportion, and then stirred evenly using a high-speed mixer.
[0017] Furthermore, in steps (1)-(2), after the bamboo fiber powder is treated with alkali, the hydroxyl groups on the fiber surface are exposed and undergo a chemical coupling reaction with the alkoxy groups in the coupling agent, thereby enhancing the interfacial compatibility between the bamboo fiber powder and the PHBH matrix.
[0018] Further, in step (3), the blend is mixed with the PHBH matrix in proportion and mixed evenly using a high-speed mixer again;
[0019] The mixture is then put into a hopper of a twin-screw extruder, wherein the temperatures of the zones of the twin-screw extruder are 140° C., 145° C., 145° C., 150° C., 150° C., 155° C., 155° C., and 160° C.;
[0020] Among them, the head temperature is 160℃ and the main engine speed is 200rpm;
[0021] The processing temperature of the melt blending process is the melt temperature in the twin-screw extruder, which is controlled at 160°C to 190°C, the stirring speed is 400 to 800 rpm, and the mixing time is 10 to 30 minutes;
[0022] After melt blending, the mixture is extruded and then pelletized using a pelletizer. The pellets are left at room temperature for 12 hours and then dried in an oven at 100°C for 24 hours. Finally, the mixture is injection molded using an injection molding machine at a temperature of 155°C.
[0023] Furthermore, by melt blending the modified bamboo fiber powder with poly (3-hydroxybutyric acid-co-3-hydroxyhexanoic acid), a series of composite materials with different mechanical properties and interface compatibility can be obtained.
[0024] The composite material significantly reduces carbon emissions while maintaining excellent biodegradability and has enhanced interface bonding force and structural stability.
[0025] Furthermore, a biodegradable composite material based on PHBH and natural plant fibers is prepared, which is suitable for manufacturing straws, packaging materials and sheet biodegradable plastic products, and has excellent mechanical properties, degradation properties and environmental protection characteristics.
[0026] In order to improve the interfacial compatibility between PHBH matrix and bamboo fiber powder and the mechanical properties of the composite material, alkali treatment can remove substances such as lignin, hemicellulose, pectin, wax and oil on the surface of plant fibers, increase the surface roughness of bamboo fiber powder, thereby increasing the contact area with the PHBH matrix and improving the interfacial bonding ability.
[0027] The alkoxy groups in the coupling agent undergo a chemical coupling reaction with the hydroxyl groups on the surface of the bamboo fiber, and the pyrophosphate groups decompose into phosphate groups when in contact with free water, further improving the interfacial bonding strength between the bamboo fiber and the PHBH matrix;
[0028] Taking a titanate coupling agent as an example, the titanate coupling agent is isopropyl tri(dioctyl pyrophosphateoxy) titanate (NDZ-201), and its molecular structure contains a pyrophosphate group;
[0029] Specifically, when it processes bamboo fiber powder, -OC3H 7 The groups can couple with the hydroxyl groups on the surface of bamboo fiber powder to reduce the surface polarity;
[0030] During the blending process, the octanoate group is entangled with the molecular chain of the PHBH matrix to enhance the bonding force between the two phases; the pyrophosphate group in the composite material not only enhances the bonding performance, improves the dispersibility and flame retardancy, but also when blended with the bamboo fiber powder, the pyrophosphate group encounters free water during the processing of the composite material and decomposes into a phosphate group. The phosphate group combines with part of the free water, thereby further ensuring the coupling effect between the coupling agent and the bamboo fiber powder, improving the interface compatibility between the matrix and the filler, and improving the mechanical properties; in addition, the addition of natural plant fibers also significantly reduces the production cost.
[0031] The invention has the beneficial effects that the main components of the composite material are all biodegradable polymer materials, which are non-toxic and environmentally friendly, can be completely degraded into carbon dioxide and water under the action of microorganisms, and have no pollution to the environment. The PHBH / bamboo fiber composite material is suitable for making plastic products such as straws, packaging materials, and plates through molding processes such as extrusion, pelletizing, injection molding, and compression molding. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a preparation flow chart of the present invention;
[0033] Figure 2 is a reaction mechanism diagram taking a titanate coupling agent as an example in an embodiment of the present invention;
[0034] Figure 3 It is a comparison diagram of the tensile section scanning electron microscope test results of Examples 1-3 and Comparative Examples 1-3 of the present invention;
[0035] Figure 4It is a comparison chart of the impact cross-section scanning electron microscope test results of Examples 1-3 and Comparative Examples 1-3 in the present invention. DETAILED DESCRIPTION
[0036] The specific technical solutions of the present invention are further described in detail below in conjunction with specific examples and the accompanying drawings.
[0037] Example 1
[0038] 425g of poly (3-hydroxybutyric acid-co-3-hydroxyhexanoic acid) (PHBH) flake solid and 75g of bamboo fiber powder pretreated with 5% alkali solution were placed in an oven and dried at 60°C for 48 hours to remove moisture. Then, the aluminate coupling agent was added to the bamboo fiber powder at a mass ratio of 3%, and a high-speed mixer was used for uniform stirring. Next, the uniformly stirred mixture of bamboo fiber and coupling agent was added to the PHBH flake solid, mixed evenly again in a high-speed mixer, and finally the mixture was put into the hopper of a twin-screw extruder. The temperature range of the twin-screw extruder was set to: 140°C, 145°C, 145°C, 150°C, 150°C, 155°C, 155°C, 160°C, 160°C, the head temperature was set to 160°C, and the main engine speed was 200rpm. After melt blending, extrusion molding is performed, and then the molded particles are pelletized using a pelletizer. The molded particles need to be placed at room temperature for 12 hours and dried in an oven at 100°C for 24 hours. Finally, the sample strips are injection molded using an injection molding machine at 155°C.
[0039] Example 2
[0040] 425g of PHBH flake solid and 75g of bamboo fiber powder pretreated with 5% alkali solution were placed in an oven and dried at 60°C for 48 hours to remove moisture. Subsequently, a titanate coupling agent was added to the bamboo fiber powder at a mass ratio of 2%, and stirred evenly using a high-speed mixer. The blend of the evenly mixed bamboo fiber and coupling agent was added to the PHBH flake solid, mixed evenly again in a high-speed mixer, and finally the mixture was put into the hopper of a twin-screw extruder, and the temperature and speed were set the same as in Example 1. After melt blending, extrusion molding was performed, and subsequent treatment was performed in the same manner.
[0041] Example 3
[0042] 425g of PHBH flake solid and 75g of bamboo fiber powder pretreated with 5% alkali solution were placed in an oven and dried at 60°C for 48 hours to remove moisture. Then, an aluminum titanate coupling agent was added to the bamboo fiber powder at a mass ratio of 4%, and stirred evenly using a high-speed mixer. The blend of the evenly mixed bamboo fiber and coupling agent was added to the PHBH flake solid, and mixed evenly again in a high-speed mixer, and finally the mixture was put into the hopper of a twin-screw extruder, and the temperature and speed were set the same as in Example 1. After melt blending, extrusion molding was performed, and subsequent treatment was performed in the same manner.
[0043] Comparative Example 1
[0044] 425g of PHBH flake solid and 75g of bamboo fiber powder were put into an oven and dried at 60°C for 48 hours to remove moisture. Then, the two were stirred evenly by a high-speed mixer to make the PHBH flake solid and bamboo fiber powder evenly mixed, and then put into the hopper of a twin-screw extruder, and the temperature of the twin-screw extruder was set to 140°C, 140°C, 140°C, 145°C, 145°C, 150°C, 150°C, 155°C, 155°C, the head temperature was set to 155°C, and the main engine speed was 200rpm. After melt blending, extrusion molding was performed, and subsequent treatment was performed in the same way.
[0045] Comparative Example 2
[0046] 425g of PHBH flake solid and 75g of bamboo fiber powder pretreated with 5% alkali solution were placed in an oven and dried at 60°C for 48 hours to remove moisture. The PHBH flake solid and bamboo fiber powder were mixed evenly using a high-speed mixer, and then put into the hopper of a twin-screw extruder, and the temperature and speed were set the same as in Example 1. After melt blending, extrusion molding was performed, and subsequent treatment was performed in the same manner.
[0047] Comparative Example 3
[0048] 425g of PHBH flake solid and 75g of bamboo fiber powder were placed in an oven and dried at 60°C for 48 hours to remove moisture. Then, a titanate coupling agent was added to the bamboo fiber powder at a mass ratio of 2%, and stirred evenly using a high-speed mixer. The blend of the bamboo fiber and the coupling agent was added to the PHBH flake solid, and mixed evenly again in a high-speed mixer. Finally, the mixture was put into the hopper of a twin-screw extruder, and the temperature and speed were set the same as in Example 1. After melt blending, extrusion molding was performed, and subsequent treatment was performed in the same manner.
[0049] Testing process and results
[0050] Mechanical properties test:
[0051] The samples were made into dumbbell-shaped splines, and the tensile properties of the dumbbell-shaped splines were tested using an electronic universal testing machine according to the standard of GB / T 1040.1-2006. Five samples were tested in each group and the average value was taken. The tensile speed was 10 mm / min. At the same time, the samples were made into rectangular splines and the unnotched impact test was carried out according to GB / T 1843-2008. The impact energy was set to 5J. Five samples were tested in each group and the average value was taken.
[0052] Scanning electron microscope test:
[0053] The fracture surfaces of the specimens pulled apart by the electronic universal testing machine and the specimens broken by the unnotched impact test were tested by scanning electron microscope to observe the surface morphology of the fracture surfaces.
[0054] Water absorption performance test:
[0055] A 2cm diameter, 2mm thick disc was prepared by vacuum molding machine. Two samples of each material were taken and the samples were fully dried at 100℃ for 24 hours. The fully dried samples were weighed and then placed in deionized water. The samples were taken out every 24 hours, the surface moisture was wiped and the sample weight was weighed. After replacing the deionized water, the samples were completely immersed again and waited for the next test.
[0056] Table 1 Mechanical properties and water absorption test results of Examples 1-3 and Comparative Examples 1-3
[0057]
Claims
1. A biodegradable composite material based on PHBH and natural plant fiber, characterized in that: The mass percentages of the components in the composite material are as follows: PHBH matrix: 80% to 85%, bamboo fiber powder: 10% to 15%, and coupling agent: 0% to 5%.
2. A biodegradable composite material based on PHBH and natural plant fibers according to claim 1, characterized in that: The mass percentages of the components in the composite material are: PHBH matrix: 85%, bamboo fiber powder: 10%, and coupling agent: 5%.
3. The biodegradable composite material based on PHBH and natural plant fibers according to claim 1, characterized in that: The bamboo fiber powder is made of natural plant fiber, which is used as a reinforcing filler and is modified by alkali treatment; The coupling agent is an additive and is selected from at least one of an aluminate coupling agent, a titanate coupling agent and an aluminum titanate coupling agent.
4. A method for preparing a biodegradable composite material based on PHBH and natural plant fibers according to any one of claims 1 to 3, characterized in that: The preparation steps are as follows: Step (1): treating the bamboo fiber powder with alkali to expose the hydroxyl groups on its surface; Step (2): adding a coupling agent to the modified bamboo fiber powder to obtain a blend of the bamboo fiber powder and the coupling agent; Step (3): The prepared blend of bamboo fiber powder and coupling agent is mixed with a PHBH matrix in proportion, and processed by a melt blending process to finally prepare a biodegradable composite material based on PHBH and natural plant fibers.
5. The method for preparing a biodegradable composite material based on PHBH and natural plant fibers according to claim 4, characterized in that: In step (1), the concentration of alkali solution required for alkali treatment of the bamboo fiber powder is 1%, 3%, 5%, 7% or 9%.
6. The method for preparing a biodegradable composite material based on PHBH and natural plant fibers according to claim 4, characterized in that: In step (1), after the bamboo fiber powder is subjected to alkali treatment, the weighed alkali-pretreated bamboo fiber powder and the prepared PHBH flake solid are placed in an oven, the temperature is set to 60° C., and dried for 48 hours to remove the remaining moisture in the PHBH flake solid.
7. The method for preparing a biodegradable composite material based on PHBH and natural plant fibers according to claim 4, characterized in that: In step (2), the coupling agent is added to the modified bamboo fiber powder in proportion, and then stirred evenly using a high-speed mixer.
8. The method for preparing a biodegradable composite material based on PHBH and natural plant fibers according to claim 4, characterized in that: In steps (1)-(2), after the bamboo fiber powder is treated with alkali, the hydroxyl groups on the fiber surface are exposed and undergo a chemical coupling reaction with the alkoxy groups in the coupling agent, thereby enhancing the interfacial compatibility between the bamboo fiber powder and the PHBH matrix.
9. The method for preparing a biodegradable composite material based on PHBH and natural plant fibers according to claim 4, characterized in that: In step (3), the blend is mixed with the PHBH matrix in proportion and mixed evenly using a high-speed mixer again; The mixture is then put into a hopper of a twin-screw extruder, wherein the temperatures of the zones of the twin-screw extruder are 140° C., 145° C., 145° C., 150° C., 150° C., 155° C., 155° C., and 160° C.; Among them, the head temperature is 160℃ and the main engine speed is 200rpm; The processing temperature of the melt blending process is the melt temperature in the twin-screw extruder, which is controlled at 160°C to 190°C, the stirring speed is 400 to 800 rpm, and the mixing time is 10 to 30 minutes; After melt blending, the mixture is extruded and then pelletized using a pelletizer. The pellets are left at room temperature for 12 hours and then dried in an oven at 100°C for 24 hours. Finally, the mixture is injection molded using an injection molding machine at a temperature of 155°C.
10. A biodegradable composite material based on PHBH and natural plant fiber prepared by the preparation method according to any one of claims 3 to 9, which is suitable for manufacturing straws, packaging materials and sheet biodegradable plastic products.