Polycarbonate composite material, display screen mask and outdoor LED display screen
By introducing components such as high-temperature resistant resin and surface modified carbon fiber into polycarbonate composite materials, the problem of thermal deformation of small-pitch outdoor LED display masks is solved, and the comprehensive performance improvement of high strength, heat resistance and weather resistance is achieved. , suitable for long-term use of small-pitch outdoor LED display screens.
Patent Information
- Application Number
- CN202411127459.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Traditional polycarbonate composite materials are prone to thermal deformation when applied to small-pitch outdoor LED displays, resulting in abnormal situations such as blocking of the display screen, black blocks or shadows, and bringing users a bad experience.
Polycarbonate composite materials that use high-temperature resistant resins and surface-modified carbon fibers to improve the strength, rigidity and heat resistance of the material through alloy modification and enhancement modification, and combine flame retardants, tougheners and weathering agents. , forming a high-performance display mask.
In an environment of 100℃ and 5000cd/m2, the monitor mask made of polycarbonate composite can work continuously for more than 4 hours, and rarely experience thermal deformation. It has significantly excellent thermal deformation resistance and is suitable for small-pitch outdoor LED display screens Long-term use.
Smart Images

Figure SMS_9 
Figure SMS_10 
Figure SMS_11
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of display, and in particular to a polycarbonate composite material, a display screen mask and an outdoor LED display screen. Background Art
[0002] Light Emitting Diode (LED) is a semiconductor electronic component that converts electrical energy into light energy. It has the advantages of energy saving, high efficiency, rich colors, fast response speed and long service life. It is widely used in lighting equipment, display screens and electronic indicator lights. Among them, large-screen display screens made of LED are mostly used in outdoor scenes such as shopping malls, high-rise buildings, and squares. In order to be suitable for long-distance viewing, a dot pitch of P6.0 or above is generally used (that is, the distance between the center points of two adjacent pixels is ≥6.0mm). With the development of application fields such as new infrastructure, smart transportation and the Internet of Things and the expansion of application scenarios, outdoor LED display screens have begun to develop towards small pitches below P4.0 to provide clearer and more delicate images.
[0003] The display screen mask is a component installed on the surface of the LED display screen module. It can prevent glare, improve contrast, improve color uniformity and provide protection. For outdoor LED displays, the protective effect of the display screen mask is particularly important. Traditional display screen masks are mostly made of polycarbonate (PC) composite materials reinforced and modified by glass fiber. However, this polycarbonate composite material is prone to deformation when applied to outdoor LED displays with small pitch, such as local bulging due to heat, obstruction of the display screen, black blocks or shadows, and other abnormal conditions, which bring a very bad experience to users. Summary of the invention
[0004] Based on this, there is a need for a polycarbonate composite material, a display screen mask and an outdoor LED display screen to solve the problem that traditional polycarbonate composite materials are prone to deformation when applied to outdoor LED displays with small pitches.
[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:
[0006] In a first aspect of the present application, a polycarbonate composite material is provided, comprising the following components in mass fractions:
[0007] ;
[0008] Wherein, the high temperature resistant resin meets the following requirements: melting point ≥ 260°C, or glass transition temperature ≥ 185°C;
[0009] The reinforcing fibers include one or more of surface-modified glass fibers and surface-modified carbon fibers;
[0010] The mass fractions of the high temperature resistant resin and the surface modified carbon fiber are not 0 at the same time.
[0011] In one embodiment, the polycarbonate composite material includes the following components in mass fractions:
[0012] .
[0013] In one embodiment, the polycarbonate composite material includes the following components in mass fractions:
[0014] ;
[0015] Wherein, the mass fraction of the surface modified carbon fiber in the polycarbonate composite material is ≥5%.
[0016] In one embodiment, the high temperature resistant resin includes one or more of liquid crystal polymer, polyphthalamide, polyetheretherketone, polyetherimide, polysulfone, polyphenylsulfone, and polyethersulfone.
[0017] In one embodiment, the surface-modified carbon fiber includes carbon fiber with a surface coated with a polymer.
[0018] In one embodiment, the polymer includes one or more of polyurethane, epoxy resin and acrylic.
[0019] In one embodiment, the mass ratio of the polymer to the carbon fiber is (1.5~6):100.
[0020] In one embodiment, the carbon fiber has a length of 4 mm to 8 mm and a diameter of 4 μm to 9 μm.
[0021] In one embodiment, the surface-modified glass fiber includes glass fiber modified by a silane coupling agent.
[0022] In one embodiment, the mass ratio of the silane coupling agent to the glass fiber is (0.5~2.5):100.
[0023] In one embodiment, the glass fiber has a length of 3 mm to 5 mm and a diameter of 8 μm to 12 μm.
[0024] In one embodiment, the toughening agent includes one or more of ethylene-methyl acrylate copolymer, methyl methacrylate-acrylate copolymer, methyl methacrylate-butadiene-styrene copolymer, ethylene-acrylate-glycidyl methacrylate terpolymer, acrylic toughening agent and acrylic-silicone rubber toughening agent;
[0025] In one embodiment, the flame retardant includes one or more of a nitrogen-based flame retardant, a phosphorus-based flame retardant, and an organic sulfonate-based flame retardant.
[0026] In one embodiment, the synergistic flame retardant includes one or more of organosiloxane, organosilicon resin, silicate and silicon powder.
[0027] In one embodiment, the weathering agent includes a light stabilizer.
[0028] In one embodiment, the polycarbonate composite material further comprises one or more of an antioxidant, a lubricant and an anti-drip agent.
[0029] In one embodiment, the antioxidant includes one or more of a hindered phenol antioxidant and a phosphite antioxidant.
[0030] In one embodiment, the lubricant includes one or more of an organosilicone polymer, a fatty acid salt, a fatty acid amide, pentaerythritol stearate, erucamide, oleamide, ethylene bisstearamide and a polyolefin wax.
[0031] In one embodiment, the anti-drip agent includes one or more of polytetrafluoroethylene, polyvinylidene fluoride and silicone.
[0032] In a second aspect of the present application, a display screen mask is provided, which is made of the polycarbonate composite material as described above.
[0033] In a second aspect of the present application, an outdoor LED display screen is provided, comprising the display screen mask as described above.
[0034] This application has at least the following beneficial effects:
[0035] The melting point of the high temperature resistant resin selected in this application is ≥260°C or the glass transition temperature is ≥185°C, which can significantly improve the strength, rigidity and heat resistance of the polycarbonate composite material, thereby reducing its thermal deformation phenomenon in high temperature environment. The glass fiber and carbon fiber in the reinforcing fiber are both surface modified, so that the reinforcing fiber and the resin have good compatibility; at the same time, compared with the glass fiber, the mechanical properties and heat resistance of the carbon fiber are better. The introduction of an appropriate amount of surface modified carbon fiber can make up for the defects of insufficient strength, rigidity and heat resistance of the composite material. This application uses high temperature resistant resin and polycarbonate for alloy modification or adds surface modified carbon fiber for reinforcement modification, and is matched with flame retardants, synergistic flame retardants, toughening agents and weathering agents in a specific ratio to greatly improve the comprehensive properties of the composite material such as strength, rigidity, heat resistance, high temperature creep resistance, flame retardancy and weather resistance. The display mask made of the polycarbonate composite material provided by this application is 100°C and 5000cd / m 2 It can work continuously for more than 4 hours in an environment with little or no bulging, and its heat-resistant deformation performance is excellent. DETAILED DESCRIPTION
[0036] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0038] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0039] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.
[0040] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0041] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.
[0042] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0043] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.
[0044] Polycarbonate (PC) is a high-performance thermoplastic engineering plastic with the advantages of high light transmittance, good weather resistance and excellent impact resistance. It can be used to prepare LED display screen masks. At present, LED display screen masks are often reinforced by adding 10wt.% of glass fiber to PC. This PC composite material can withstand high temperatures of 40℃~60℃. For LED display screen masks with a dot pitch of P6.0 or above, due to the relatively large rib size and thickness of the product, traditional PC composite materials do not produce obvious thermal deformation when used in outdoor scenes for a long time. However, for LED display screen masks with a dot pitch below P4.0, the display brightness exceeds 4500cd / m 2When the temperature of the display screen surface exceeds 60℃ or even reaches above 80℃ under extreme conditions, the display screen surface temperature will exceed 60℃ or even reach above 80℃. At this time, if the display screen continues to use traditional PC composite materials, obvious thermal deformation will occur, which will directly manifest as local bulging due to heat, the display screen will be blocked, and abnormal conditions such as black blocks or shadows will be generated, which will bring a very bad experience to users.
[0045] There are reports on a method for making a small-pitch mask for an outdoor LED display screen, which uses 70wt.%~80wt.% polyphenylene sulfide as the base material and adds 20wt.%~30wt.% glass fiber for blending modification. Although this composite material can improve the mask bulging problem, the material cost is high and the detailed structure of the mask needs to be optimized, which further increases the cost. Therefore, it is necessary to develop a composite material with high strength, high modulus, excellent heat resistance and low cost, which can effectively solve the problem of thermal deformation of small-pitch outdoor LED display screen masks while keeping the product structure unchanged.
[0046] Based on this, in a first aspect, the present application provides a polycarbonate composite material.
[0047] In some embodiments, the polycarbonate composite material includes the following components in mass fractions:
[0048] ;
[0049] Among them, the high temperature resistant resin meets the following requirements: melting point ≥ 260°C, or glass transition temperature ≥ 185°C;
[0050] The reinforcing fibers include one or more of surface-modified glass fibers and surface-modified carbon fibers;
[0051] The mass fractions of the high temperature resistant resin and the surface modified carbon fiber are not the same and are 0.
[0052] The melting point of the high temperature resistant resin selected in this application is ≥260°C or the glass transition temperature is ≥185°C, which can significantly improve the strength, rigidity and heat resistance of the polycarbonate composite material, thereby reducing its thermal deformation phenomenon in high temperature environment. The glass fiber and carbon fiber in the reinforcing fiber are both surface modified, so that the reinforcing fiber and the resin have good compatibility; at the same time, compared with the glass fiber, the mechanical properties and heat resistance of the carbon fiber are better. The introduction of an appropriate amount of surface modified carbon fiber can make up for the defects of insufficient strength, rigidity and heat resistance of the composite material. This application uses high temperature resistant resin and polycarbonate for alloy modification or adds surface modified carbon fiber for reinforcement modification, and is matched with flame retardants, synergistic flame retardants, toughening agents and weathering agents in a specific ratio to greatly improve the comprehensive properties of the composite material such as strength, rigidity, heat resistance, high temperature creep resistance, flame retardancy and weather resistance. The display mask made of the polycarbonate composite material provided by this application is 100°C and 5000cd / m 2 It can work continuously for more than 4 hours in an environment with little or no bulging, and its heat-resistant deformation performance is excellent.
[0053] As an example, the mass fraction of polycarbonate (PC) in the PC composite material may be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70% or 75%.
[0054] As an example, the mass fraction of the high temperature resistant resin in the PC composite material can be 0%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%.
[0055] As an example, the mass fraction of reinforcing fibers in the PC composite material can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%.
[0056] As an example, the mass fraction of the flame retardant in the PC composite material can be 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5% or 12%.
[0057] As an example, the mass fraction of the synergistic flame retardant in the PC composite material can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%.
[0058] As an example, the mass fraction of the toughening agent in the PC composite material can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%.
[0059] As an example, the mass fraction of the weathering agent in the PC composite material can be 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55% or 0.6%.
[0060] Optionally, the polycarbonate composite material includes the following components in mass fractions:
[0061] .
[0062] In this application, if a high temperature resistant resin with a mass fraction of 40% to 45% is added to PC for blending and modification, the strength, rigidity and heat resistance of the PC composite material can be greatly improved regardless of whether the reinforcing fiber contains surface modified carbon fiber. When the content of high temperature resistant resin is the same, replacing part or all of the surface modified glass fiber with surface modified carbon fiber can obtain higher strength, rigidity and heat resistance.
[0063] As an example, the mass fraction of PC in the PC composite may be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%.
[0064] As an example, the mass fraction of the high temperature resistant resin in the PC composite material can be 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5% or 45%.
[0065] Optionally, the polycarbonate composite material includes the following components in mass fractions:
[0066] ;
[0067] Among them, the mass fraction of the surface modified carbon fiber in the polycarbonate composite material is ≥5%.
[0068] In this application, without adding high temperature resistant resin, adding surface modified carbon fiber with a mass fraction of ≥5% can also significantly improve the strength, rigidity and heat resistance of PC composite materials.
[0069] As an example, the mass fraction of PC in the PC composite may be 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74% or 75%.
[0070] As an example, the mass fraction of the surface modified carbon fiber in the PC composite material is 5% to 20%, for example 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%.
[0071] As an example, the mass fraction of the surface modified glass fiber in the PC composite material is 0% to 15%, for example, 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%.
[0072] Optionally, the synthesis process of PC includes one or more of non-phosgene method, semi-phosgene method and phosgene method. Among them, the main raw materials of the phosgene method are bisphenol A and GAC, and its process is relatively mature, which is conducive to the production of high molecular weight PC. Therefore, this application selects phosgene method PC with higher molecular weight.
[0073] Optionally, PC meets the following conditions: the number average relative molecular weight is 20000-50000; the melt flow index (MFI) at a temperature of 300° C. and a load of 1.2 kg is ≥10 g / 10 min.
[0074] In this application, the high temperature resistant resin can be divided into three types according to different resin compositions: crystalline, semi-crystalline and amorphous. For crystalline and semi-crystalline high temperature resistant resins, their melting points (Melting Point, T m ) should be above 260℃. For non-crystalline high temperature resistant resin, its glass transition temperature (Glass Transition Temperature, T g ) should be above 185℃.
[0075] Optionally, the high temperature resistant resin includes one or more of liquid crystal polymer, polyphthalamide, polyetheretherketone, polyetherimide, polysulfone, polyphenylsulfone, and polyethersulfone. Further optionally, the high temperature resistant resin includes one or more of polyetherimide, polysulfone, polyphenylsulfone, and polyethersulfone.
[0076] The high temperature resistant resin selected in this application has a similar bisphenol A structure to PC, so that the high temperature resistant resin has a certain compatibility with PC at different dosages, thus showing a good alloy modification effect. Among them, Liquid Crystal Polymer (LCP) is a polymer material with special properties. It not only has high strength, high modulus, good tensile and bending resistance, but also excellent heat resistance and can maintain stable performance at higher temperatures. Polyphthalamide (PPA) has two forms: semi-crystalline and amorphous. The melting point of its semi-crystalline state is about 310°C. It has excellent heat resistance and also performs well in high temperature creep resistance, fatigue resistance and chemical resistance. Polyetheretherketone (PEEK) has excellent high temperature resistance, and the long-term use temperature can reach 260°C. It also has high strength, high modulus and good chemical corrosion resistance. Polyetherimide (PEI) is an amorphous high-performance thermoplastic with excellent heat resistance, a glass transition temperature of up to 217°C, a long-term use temperature of over 170°C, high strength, high rigidity, excellent flame retardancy and excellent chemical corrosion resistance. Polysulfone (PSU) is a high-performance thermoplastic with good heat resistance and a long-term use temperature of 150°C to 174°C. It also has high strength, high rigidity, high transparency, good chemical corrosion resistance and good dimensional stability, and its size changes very little under different temperature and humidity conditions. Polyphenylsulfone (PPSU) is a high-performance special engineering plastic with excellent high temperature resistance and can maintain stable performance over a wide temperature range. The long-term use temperature can reach over 180°C. It also has excellent mechanical strength, superior chemical corrosion resistance and good dimensional stability. Polyethersulfone (PES) is a special engineering plastic with excellent performance and outstanding heat resistance. The long-term use temperature can reach 180°C and the short-term use temperature can even exceed 220°C. It also has the advantages of high strength and rigidity, excellent chemical corrosion resistance, good dimensional stability and high transparency.
[0077] It is understandable that the present application does not specifically limit the particle size of the high temperature resistant resin. Usually, the high temperature resistant resin exists in the form of flakes or powders, which can be made into granules and then blended with PC for alloy modification. However, powdered PEEK is difficult to process into granules.
[0078] Optionally, the surface-modified carbon fibers include carbon fibers whose surfaces are coated with a polymer.
[0079] Optionally, the polymer includes one or more of polyurethane, epoxy resin and acrylic acid. Further optionally, the polymer coated on the surface of the carbon fiber is epoxy resin; or, the polymer coated on the surface of the carbon fiber is acrylic acid and polyurethane, and the mass ratio of acrylic acid to polyurethane is (1-2):(2-1). As an example, the mass ratio of acrylic acid to polyurethane can be 1:1, 1:1.5, 1:2, 2:1 or 2:1.5, and can further be 1:2.
[0080] In the present application, coating the surface of carbon fiber with polymers such as polyurethane, epoxy resin and acrylic acid can enhance the compatibility between carbon fiber and resin, avoid the defect of unsatisfactory enhancement modification effect due to poor compatibility, and play an important role in improving the strength, rigidity and heat resistance of composite materials.
[0081] Optionally, the mass ratio of the polymer to the carbon fiber is (1.5-6): 100, and further optionally (2.5-4.5): 100. As an example, the mass ratio of the polymer to the carbon fiber can be 1.5: 100, 2: 100, 2.5: 100, 3: 100, 3.5: 100, 4: 100, 4.5: 100, 5: 100, 5.5: 100 or 6: 100.
[0082] Optionally, the length of the carbon fiber is 4 mm to 8 mm, and the diameter is 4 μm to 9 μm. Further optionally, the length of the carbon fiber is 5 mm to 7 mm, and the diameter is 6 μm to 8 μm. As an example, the length of the carbon fiber can be 4 mm, 4.5 mm, 5 mm, 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, or 8 mm, and the diameter can be 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, or 9 μm.
[0083] Optionally, the surface-modified glass fiber includes glass fiber modified with a silane coupling agent.
[0084] In the present application, the surface of the glass fiber is modified by a silane coupling agent, which can enhance the compatibility between the glass fiber and the resin, avoid the defect of unsatisfactory enhancement and modification effect due to poor compatibility, and play an important role in improving the strength, rigidity and heat resistance of the composite material.
[0085] Optionally, the mass ratio of the silane coupling agent to the glass fiber is (0.5-2.5): 100. As an example, the mass ratio of the silane coupling agent to the glass fiber can be 0.5:100, 0.8:100, 1:100, 1.2:100, 1.5:100, 1.8:100, 2:100, 2.2:100, 2.4:100 or 2.5:100.
[0086] Optionally, the glass fiber is a long glass fiber or a chopped glass fiber, and the length of the glass fiber is 3 mm to 5 mm, and the diameter is 8 μm to 12 μm. As an example, the length of the glass fiber can be 3 mm, 3.2 mm, 3.8 mm, 3.8 mm, 4 mm, 4.2 mm, 4.5 mm, 4.8 mm, or 5 mm, and the diameter can be 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11 μm, 11.5 μm, or 12 μm.
[0087] Optionally, the toughening agent includes one or more of ethylene-methyl acrylate copolymer, methyl methacrylate-acrylate copolymer, methyl methacrylate-butadiene-styrene copolymer, ethylene-acrylate-glycidyl methacrylate terpolymer, acrylic toughening agent and acrylic-silicone rubber toughening agent, and further can be selected from one or more of methyl methacrylate-butadiene-styrene copolymer, ethylene-acrylate-glycidyl methacrylate terpolymer and acrylic-silicone rubber toughening agent.
[0088] The toughening agent selected in the present application has an acrylic acid functional group or an acrylate functional group, has a certain polarity and an active functional group, can play a role at the interface of polymers of different polarities, enhance the interfacial bonding force, and help improve compatibility while toughening, reduce phase separation, and improve the performance of the alloy modified material.
[0089] Optionally, the flame retardant includes one or more of nitrogen flame retardant, phosphorus flame retardant and organic sulfonate flame retardant, and further phosphorus flame retardant can be selected. Among them, nitrogen flame retardant includes one or more of melamine, melamine cyanurate, melamine phosphate, dicyandiamide and guanidine compounds; phosphorus flame retardant includes one or more of triphenyl phosphate, bisphenol A-bis (diphenyl phosphate) and resorcinol-bis (diphenyl phosphate); organic sulfonate flame retardant includes one or more of sodium 2,4,5-trichlorobenzenesulfonate, potassium benzenesulfonylbenzenesulfonate and potassium perfluorobutyl sulfonate.
[0090] Optionally, the synergistic flame retardant includes one or more of organic siloxane, organic silicone resin, silicate, and silicon powder, and may further be organic siloxane.
[0091] In this application, synergistic flame retardant refers to an auxiliary agent that can significantly improve the flame retardant effect and reduce the amount of the main flame retardant when used in combination with the main flame retardant in the flame retardant system. Among them, organosiloxane synergistic flame retardants can assist in flame retardancy by promoting charring and releasing inert gases. They have good thermal stability, low smoke and low toxicity, and can improve the processability and fluidity of composite materials. The coordinated use of organosiloxane synergistic flame retardants and phosphorus flame retardants can make PC composite materials achieve good flame retardant effects and maintain good mechanical strength and high transparency.
[0092] Optionally, the weathering agent includes a light stabilizer.
[0093] It can be understood that light stabilizers are a class of additives that can inhibit or slow down the degradation and aging of polymer materials under the action of light (mainly ultraviolet rays), usually including one or more of ultraviolet absorbers, free radical scavengers and quenchers. Among them, ultraviolet absorbers are a class of additives that can absorb ultraviolet rays to protect materials from ultraviolet damage. Common ones include benzophenones, benzotriazoles and triazines. Free radical scavengers are a class of substances that can effectively capture and terminate free radical chain reactions, and play an important role in preventing material aging and degradation. Common ones include hindered amine compounds such as piperidine derivatives and imidazoline derivatives, as well as phenolic compounds such as butylated hydroxyanisole (BHA) and dibutyl hydroxytoluene (BHT). Quenchers are a class of substances that can return excited molecules to the ground state through energy transfer or charge transfer, thereby reducing the probability of photochemical reactions. Common ones include metal ion quenchers and aromatic quenchers.
[0094] Optionally, the weathering agent includes an ultraviolet absorber and a free radical scavenger. The ultraviolet absorber includes one or more of a benzotriazole ultraviolet absorber and a triazine ultraviolet absorber; the free radical scavenger includes a hindered amine free radical scavenger; and the mass ratio of the ultraviolet absorber to the free radical scavenger is (1-3):(1-3), for example, 1:1, 2:1, 3:1, 1:2, 3:2, 1:3 or 2:3.
[0095] Optionally, the polycarbonate composite material further comprises one or more of an antioxidant, a lubricant and an anti-drip agent.
[0096] Optionally, the polycarbonate composite material further comprises the following components in mass fractions:
[0097] .
[0098] As an example, the mass fraction of the antioxidant in the PC composite material can be 0.3%, 0.4%, 0.5%, 0.6%; the mass fraction of the lubricant in the PC composite material is 0.4%, 0.5%, 0.6%, 0.7% or 0.8%; the mass fraction of the anti-dripping agent in the PC composite material is 0%, 0.1%, 0.2%, 0.3%, 0.4% or 0.5%.
[0099] Optionally, the antioxidant includes one or more of a hindered phenol antioxidant and a phosphite antioxidant. Further optionally, the mass ratio of the hindered phenol antioxidant to the phosphite antioxidant is (1-2):(1-4), such as 1:1, 2:1, 1:2, 1:3, 2:3 or 1:4.
[0100] Optionally, the lubricant includes one or more of organic silicone polymers, fatty acid salts, fatty acid amides, pentaerythritol stearate, erucamide, oleamide, ethylene bisstearamide and polyolefin wax, and further optionally one or more of organic silicone polymers, pentaerythritol stearate and ethylene bisstearamide.
[0101] Optionally, the anti-drip agent includes one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF) and silicone, and may further be polytetrafluoroethylene (PTFE).
[0102] In some embodiments, the method for preparing the PC composite material comprises the following steps:
[0103] S100: Mix PC, high temperature resistant resin, flame retardant, synergistic flame retardant, toughening agent and weathering agent to prepare a blend;
[0104] S200: mixing the blend and the reinforcing fiber, performing extrusion molding treatment, and preparing a molding material;
[0105] S300: granulating the molding material to prepare a PC composite material.
[0106] Optionally, the blend also contains one or more of an antioxidant, a lubricant, and an anti-drip agent.
[0107] Optionally, in the mixing process of step S100, the mixing equipment is a high-speed mixing stirrer, the stirring speed is 400 rpm to 800 rpm, and the stirring time is 2 min to 3 min.
[0108] Optionally, in the extrusion process of step S200, the extrusion equipment is a screw extruder, the blend enters the extruder through a hopper, and the reinforcing fiber enters the extruder through a side feeder. The main engine feeding speed is 15rpm~25rpm, and the side feeder feeding speed is 8rpm~15rpm; the extrusion temperature is 250℃~290℃, the screw speed is 350rpm~450rpm, and the vacuum degree is -0.02MPa~-0.04MPa.
[0109] Optionally, the granulation process of step S300 includes processes such as die, strand drawing and pelletizing.
[0110] Optionally, the particle size of the PC composite material is 1.5 mm to 4.0 mm, for example, 1.5 mm, 1.8 mm, 2 mm, 2.2 mm, 2.5 mm, 2.8 mm, 3 mm, 3.2 mm, 3.5 mm, 3.8 mm or 4 mm.
[0111] Optionally, the tensile strength of the PC composite material is ≥72 MPa, and can further be 100 MPa~120 MPa.
[0112] Optionally, the flexural modulus of the PC composite material is ≥3700 MPa, and further optionally is 4600 MPa~7000 MPa.
[0113] Optionally, the notched cantilever impact strength of the PC composite material is ≥6 kJ / m 2 , further optional to 6.4kJ / m 2 ~10kJ / m 2 .
[0114] Optionally, the heat deformation temperature of the PC composite material is ≥150°C, and can further be 153°C~160°C.
[0115] Optionally, the flame retardant grade of the PC composite material is V0 at a thickness of 1.6 mm.
[0116] In a second aspect of the present application, a display screen mask is provided, which is made of the polycarbonate composite material as described above.
[0117] Optionally, the display screen mask is at a temperature of 100°C and a brightness of 5000cd / m 2 When working continuously for more than 4 hours in an environment, the number of bulges or shadows on the surface shall not exceed 3.
[0118] In a third aspect of the present application, an outdoor LED display screen is provided, comprising the display screen mask as described above.
[0119] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0120] Example 1
[0121] Please refer to Table 1, the PC composite material of this embodiment is composed of the following components by mass fraction: .
[0122] Among them, the high temperature resistant resin is polyethersulfone (PES); the surface modified glass fiber is a glass fiber modified by a silane coupling agent, the length of the glass fiber is 3mm~5mm, and the fiber diameter is 8μm~12μm; the flame retardant is bisphenol A diphenyl phosphate, the synergistic flame retardant is polysiloxane, the toughening agent is ethylene-acrylate-methacrylate glycidyl ester terpolymer, the weathering agent is benzotriazole UV234, the antioxidant is a compound of hindered phenol 1076 main antioxidant and phosphite 168 auxiliary antioxidant, the lubricant is pentaerythritol stearate, and the anti-dripping agent is polytetrafluoroethylene powder.
[0123] The preparation method of the PC composite material of this embodiment is as follows:
[0124] (1) PC, high temperature resistant resin, flame retardant, synergistic flame retardant, toughening agent, weathering agent, antioxidant, lubricant and anti-dripping agent are placed in a high-speed mixer and stirred at a stirring speed of 400 rpm to 800 rpm for 2 min to 3 min to obtain a uniformly mixed blend.
[0125] (2) The blend is fed into the extruder through a hopper, and the feeding speed is controlled at 15 rpm to 25 rpm; the reinforcing fiber is fed into the extruder through a side feeder, and the feeding speed is 8 rpm to 15 rpm; the extrusion temperature is set to 250°C to 290°C, the screw speed is set to 350 rpm to 450 rpm, and the vacuum degree is set to -0.02 MPa to -0.04 MPa, and extrusion molding is performed to obtain a molding material.
[0126] (3) The molding material is granulated through processes such as die, strip drawing and pelletizing to obtain a PC composite material with a particle size of 1.5 mm to 4.0 mm.
[0127] Embodiment 2~6
[0128] The formulas of the PC composite materials of Examples 2 to 6 are detailed in Table 1, and the preparation methods thereof are the same as that of Example 1.
[0129] Among them, Examples 1 to 4 added high temperature resistant resin polyethersulfone (PES), Examples 1 to 2 did not add surface modified carbon fiber, Examples 3 to 4 added surface modified carbon fiber; Examples 5 to 6 did not add poly high temperature resin, but added surface modified carbon fiber.
[0130] Comparative Examples 1 to 4
[0131] The formulas of the PC composite materials of Comparative Examples 1 to 4 are detailed in Table 1, and the preparation methods thereof are the same as that of Example 1.
[0132] Among them, comparative example 1 did not add poly-high temperature resin and surface modified carbon fiber;
[0133] Comparative Example 2 is substantially the same as Example 4, except that no toughening agent is added;
[0134] Comparative Example 3 is substantially the same as Example 3, except that the surface-modified carbon fiber is replaced with carbon fiber that is not surface-modified;
[0135] Comparative Example 4 is substantially the same as Example 2, except that the surface-modified glass fiber is replaced by glass fiber that is not surface-modified.
[0136] Test Case
[0137] The PC composite materials in each embodiment and each comparative example were injection molded to prepare standard specimens and display masks according to standard requirements. The performance of the PC composite materials was tested according to standard methods, and the results are shown in Table 2. The display mask was assembled into an LED box, and the LED box was tested as follows, and the results are shown in Table 3.
[0138] (1) Tensile strength: refer to GB / T 1040.1-2018 Determination of tensile properties of plastics;
[0139] (2) Elongation at break: refer to GB / T 1040.1-2018 Determination of tensile properties of plastics;
[0140] (3) Flexural modulus: Refer to GB / T 9341-2000 Test method for flexural properties of plastics
[0141] (4) Izod notched impact strength: refer to GB / T 1843-2008 Determination of cantilever beam impact strength of plastics;
[0142] (5) Heat deformation temperature: refer to GB / T 1634.1-2019 Determination of load deformation temperature of plastics;
[0143] (6) Flame retardant grade: refer to UL 94 flame retardant grade standard.
[0144] (7) LED cabinet heating aging test: Place the LED cabinet in an oven and perform cabinet lighting and aging tests at 40℃, 50℃, 60℃, 70℃, 80℃, 90℃ and 100℃ in sequence. According to the serial conditions, at each temperature, 5000cd / m 2 Brightness: light up for at least 4 hours. When the number of bulges or shadows exceeds 15 per cabinet, stop verification and record the temperature when verification is stopped. The results are shown in Table 3.
[0145] As can be seen from Tables 1 to 3, Examples 1 to 2 use high temperature resistant resin and PC for alloy modification, Examples 5 to 6 use surface modified carbon fiber to enhance polycarbonate, and Examples 3 to 4 use both of the above modification treatments, which can greatly improve the strength, rigidity and heat resistance of PC composite materials. In the temperature rise aging test of the LED box, the mask made of the PC composite material of Examples 1 to 6 rarely or even does not have bulging defects, indicating that it has excellent heat deformation resistance and is very suitable for long-term use in small-pitch outdoor LED display screens.
[0146] Table 1. PC composite material formula (unit: wt.%)
[0147]
[0148] Table 2. Performance comparison of PC composite materials
[0149]
[0150] Table 3. LED cabinet temperature rise aging test results
[0151]
[0152] Note: “--” in Table 3 means verification has been stopped.
[0153] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0154] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.
Claims
1. A polycarbonate composite material, characterized in that: The components include the following mass fractions: ; Wherein, the high temperature resistant resin meets the following requirements: melting point ≥ 260°C, or glass transition temperature ≥ 185°C; The reinforcing fibers include one or more of surface-modified glass fibers and surface-modified carbon fibers; The mass fractions of the high temperature resistant resin and the surface modified carbon fiber are not 0 at the same time.
2. The polycarbonate composite material according to claim 1, characterized in that: The polycarbonate composite material comprises the following components by mass fraction: 。 3. The polycarbonate composite material according to claim 1, characterized in that: The polycarbonate composite material comprises the following components by mass fraction: ; Wherein, the mass fraction of the surface modified carbon fiber in the polycarbonate composite material is ≥5%.
4. The polycarbonate composite material according to any one of claims 1 to 3, characterized in that: The high temperature resistant resin includes one or more of liquid crystal polymer, polyphthalamide, polyetheretherketone, polyetherimide, polysulfone, polyphenylsulfone and polyethersulfone.
5. The polycarbonate composite material according to claim 4, characterized in that: The surface-modified carbon fiber includes a carbon fiber with a polymer coated on the surface, and satisfies one or more of the following conditions: (1) The polymer includes one or more of polyurethane, epoxy resin and acrylic acid; (2) The mass ratio of the polymer to the carbon fiber is (1.5-6):100; (3) The length of the carbon fiber is 4 mm to 8 mm, and the diameter is 4 μm to 9 μm.
6. The polycarbonate composite material according to claim 4, characterized in that: The surface-modified glass fiber includes a glass fiber modified by a silane coupling agent, and satisfies one or more of the following conditions: (1) The mass ratio of the silane coupling agent to the glass fiber is (0.5-2.5):100; (2) The length of the glass fiber is 3 mm to 5 mm, and the diameter is 8 μm to 12 μm.
7. The polycarbonate composite material according to claim 4, characterized in that: One or more of the following conditions are met: (1) The toughening agent includes one or more of ethylene-methyl acrylate copolymer, methyl methacrylate-acrylate copolymer, methyl methacrylate-butadiene-styrene copolymer, ethylene-acrylate-glycidyl methacrylate terpolymer, acrylic toughening agent and acrylic-silicone rubber toughening agent; (2) The flame retardant includes one or more of a nitrogen-based flame retardant, a phosphorus-based flame retardant and an organic sulfonate-based flame retardant; (3) The synergistic flame retardant includes one or more of organosiloxane, organosilicon resin, silicate and silicon powder; (4) The weathering agent includes a light stabilizer.
8. The polycarbonate composite material according to claim 4, characterized in that: The polycarbonate composite material further comprises one or more of an antioxidant, a lubricant and an anti-drip agent, and satisfies one or more of the following conditions: (1) The antioxidant includes one or more of a hindered phenol antioxidant and a phosphite antioxidant; (2) The lubricant includes one or more of organosiloxane polymers, fatty acid salts, fatty acid amides, pentaerythritol stearate, erucamide, oleamide, ethylene bisstearamide and polyolefin wax; (3) The anti-dripping agent includes one or more of polytetrafluoroethylene, polyvinylidene fluoride and silicone.
9. A display screen mask, characterized in that: The polycarbonate composite material is made of the polycarbonate composite material as described in any one of claims 1 to 8.
10. An outdoor LED display screen, characterized in that: Comprising the display screen mask as claimed in claim 9.
Citation Information
Patent Citations
Modified polycarbonate composition and LED (light-emitting diode) full-color screen module mask prepared therefrom
CN102964792A
Glass fiber reinforced polycarbonate (PC) composite material and preparation method thereof
CN104672849A
Glass fiber reinforced halogen-free flame retardant PC (polycarbonate) / PEI (polyetherimide) composite material and preparation method thereof
CN104672882A
Preparation method of high-temperature-resistant reinforced PC composite material
CN110922736A
Polycarbonate composition with high heat resistance and impact resistance and preparation method thereof
CN111057358A
Cited By
Composite material, preparation method and application thereof and three-dimensional space additive manufacturing product
CN120718446A
PC (polycarbonate) composition as well as preparation method and application thereof
CN120888173A
Polycarbonate composite material, display mask, and outdoor LED display
WO2026036946A1