High-temperature-resistant glass fiber composite material and preparation method thereof

Through the cross-linking reaction of end-alkenyl unsaturated polyamide with glass fiber, silicone raw glue and hydrogen-containing silicone oil, combined with heat cross-linking technology, the moisture absorption and interface of glass fiber reinforced nylon materials under high temperature and high humidity conditions is solved. Compatibility issues enable high-strength, hydrophobic, moisture-proof and high-temperature-resistant glass fiber composite materials.

CN119081397AInactive Publication Date: 2024-12-06NANTONG QIANGZHENG COMPOSITE MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411422231.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing glass fiber reinforced nylon materials are prone to moisture absorption and hydrolysis under high temperature and high humidity conditions, and there is an interface compatibility problem between glass fiber and polyamide chain, resulting in insufficient material performance.

Method used

The cross-linking reaction of end-alkenyl unsaturated polyamide is carried out with glass fiber, vinyl silicone raw glue and hydrogen-containing silicone oil to form a mutual transmission network structure. Combined with the heat cross-linking process, glass fiber is directly added to reduce the interface effect, and The molding is performed by controlling the viscosity.

Benefits of technology

It significantly improves the hydrophobicity, moisture resistance and high temperature resistance of the material, and at the same time improves the distribution uniformity and strength of glass fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant glass fiber composite material and a preparation method thereof. The high-temperature-resistant glass fiber composite material comprises alkenyl-terminated unsaturated polyamide, glass fibers, vinyl siloxane raw rubber, hydrogen-containing silicone oil, a Pt catalyst and an inhibitor. The preparation method comprises the steps of preparation of terminal alkenyl unsaturated polyamide, silica gel mixing, pre-crosslinking reaction, forming and the like. According to the invention, primary amino and terminal NCO are subjected to a reaction to prepare unsaturated polyamide with terminal alkenyl branched chains, then hydrogen-containing silicone oil is subjected to a cross-linking reaction with the terminal alkenyl unsaturated polyamide and vinyl siloxane raw rubber, and the glass fibers are directly added in the thermal cross-linking process, so that the glass fiber reinforced thermoplastic elastomer is obtained. Therefore, the glass fiber and a cross-linking system form an intertransmission network structure, the interface effect is avoided, the glass fiber is uniformly distributed, a large amount of silica gel is contained to coat and block holes, the surface hydrophobicity and moisture resistance are greatly improved, and a hydrophobic, moisture-proof, high-temperature-resistant and high-strength glass fiber product is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high temperature resistant materials, and in particular to a high temperature resistant glass fiber composite material and a preparation method thereof. Background Art

[0002] Glass fiber reinforced plastics are made by adding glass fiber and other additives to the original pure plastics, thereby increasing the scope of use of the materials. Glass fiber reinforced materials include glass fiber reinforced PP, glass fiber reinforced ABS, glass fiber reinforced AS, glass fiber reinforced PA66, glass fiber reinforced PA6, glass fiber reinforced PC, etc. For example, glass fiber reinforced tanks used to load various media are made of synthetic resin as the matrix and glass fiber reinforced materials, which are specially used for treating domestic sewage and recycling natural precipitation.

[0003] FRP tanks with glass fiber reinforced nylon materials have high heat resistance, rigidity, strength, impact resistance and flame retardancy. However, due to the water absorption of the amide group and the hollow structure of the glass fiber itself, the material is easy to absorb moisture. Nylon is prone to hydrolysis under high temperature and high humidity conditions. In addition, there are certain interface compatibility issues between glass fiber and polyamide chains, which need to be improved. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high temperature resistant glass fiber composite material and a preparation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A high temperature resistant glass fiber composite material comprises the following components in parts by weight: 100 parts of terminal ethylenically unsaturated polyamide, 30-35 parts of glass fiber, 15-20 parts of vinyl silicone rubber, 2-5 parts of hydrogen silicone oil, 0.8-0.9 parts of Pt catalyst, 0.002-0.003 inhibitor.

[0006] Preferably, the preparation process of the terminal ethylenically unsaturated polyamide is as follows: 960g of adipic acid and 1050g of polyetheramine were placed in a reactor under a nitrogen atmosphere, and the reactor was heated to 170°C until the amine value dropped below 0.1mg / g. 135g of diethanolamine was first added dropwise using a dropping funnel and reacted for 1h, and then 200g of ethanolamine was added dropwise. The mixture was then reacted at 170°C for 3h, and the temperature was lowered to maintain 120°C for dehydration for 30min. After the dehydration was completed, the temperature was lowered to below 60°C, 400g of ethyl isocyanate acrylate (excessive) was added, and the temperature was raised to 80°C to obtain a viscous liquid, thereby generating a polyamide system containing terminal NCO. 50 g of allylamine was added to the viscous liquid, and the reaction was continued at 80° C. under nitrogen protection for 2 hours to obtain a viscous and transparent terminal ethylenically unsaturated polyamide.

[0007] Preferably, the vinyl silicone rubber is a polysiloxane with vinyl short-circuits at both ends of the molecular chain, is in liquid form, has a molecular weight of 15,000, and a vinyl content of 0.015 to 0.02 mmol vinyl / g vinyl silicone rubber.

[0008] Preferably, the hydrogen-containing silicone oil comprises at least one polydimethyl silicone oil with Si-H bonds, and contains at least 3 silicon-hydrogen bonds on the molecular chain. The hydrogen content of the hydrogen-containing silicone oil is between 1.1 and 1.3 mmol / g.

[0009] Preferably, the Pt catalyst is a Custer catalyst platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, which is a colorless to pale yellow liquid with a viscosity of 800 to 1000 mPa.s and a boiling point of 132 to 135°C, and can volatilize and leave the silicone tube system during high-temperature vulcanization.

[0010] Preferably, the inhibitor is 1-ethynylcyclohexanol or vinylmethylcyclosiloxane, which is used to inhibit or delay the hydrosilation reaction.

[0011] The present invention also provides a method for preparing the aforementioned high temperature resistant glass fiber composite material, comprising the following steps: S1, Silicone Mix Put terminal ethylenically unsaturated polyamide, glass fiber, vinyl silicone rubber, hydrogenated silicone oil, Pt catalyst and inhibitor into an internal mixer according to a weight ratio of 100:30-35:15-20:2-5:0.8-0.9:0.002-0.003, and mix for 30 minutes at a mixing temperature of 15-20°C; S2. Pre-crosslinking reaction Increase the temperature of the internal mixer to 180-200°C, continue mixing for 30 minutes, stop stirring, and the system viscosity increases to 10000-12000cps; S3, Forming The mixed system obtained in S2 is put into an extrusion film-forming machine, the temperatures of zones 1-3 are 180°C, 210°C, and 250°C respectively, the outlet pressure is 10MPa, the cooling temperature is 20-30°C, and it is formed into a thin strip and curled to obtain a finished high-temperature resistant glass fiber composite material.

[0012] The high temperature resistant glass fiber composite material product obtained by the preparation method is used in the preparation of glass fiber reinforced plastic tanks. The high temperature resistant glass fiber composite material product is wound into a blank, subjected to high temperature pressure holding and shaping for 30 minutes at 250° C., and then cooled under pressure to obtain a glass fiber reinforced plastic tank.

[0013] GB / T 8237-1987 "Liquid unsaturated polyester resin for glass fiber reinforced plastics (FRP)" Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses a primary amine group to react with a terminal NCO to prepare an unsaturated polyamide with a terminal olefinic branch, and then uses a cross-linking reaction between hydrogen-containing silicone oil and the terminal olefinic unsaturated polyamide and vinyl silicone rubber to obtain a silicone polyamide composite material with good waterproof performance and high temperature resistance.

[0014] 2. The present invention divides the thermal cross-linking reaction into two parts, and directly adds glass fiber during the thermal cross-linking process, so that the glass fiber and the cross-linking system form an interconductive network structure with no interface effect. The glass fiber is evenly distributed and contains a large amount of silica gel coating to plug the pores, which greatly improves the surface hydrophobicity and moisture resistance.

[0015] 3. The present invention controls the viscosity of the pre-crosslinked mixing to obtain an extruded blank. On the basis of satisfying the processing and molding requirements, the three originally incompatible materials, polyamide, silica gel and glass fiber, are combined together through thermal crosslinking to obtain a hydrophobic, moisture-proof, high-temperature resistant and high-strength glass fiber product. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.

[0017] Preparation Example 1: The preparation process of the terminal olefinically unsaturated polyamide is as follows: Referring to patent CN 111635521 B "A hydroxy-terminated unsaturated polyamide and its preparation method and application", 960g of adipic acid and 1050g of polyetheramine were placed in a reactor under a nitrogen atmosphere, and the reactor was heated to 170°C until the amine value dropped below 0.1mg / g. 135g of diethanolamine was first added dropwise with a dropping funnel and reacted for 1h, and then 200g of ethanolamine was added dropwise; the mixture was then reacted at 170°C for 3h, cooled and maintained at 120°C for dehydration for 30min, and after the dehydration was completed, the temperature was lowered to below 60°C, 400g of isocyanate ethyl acrylate (excessive) was added, and the temperature was raised to 80°C to obtain a viscous liquid, thereby generating a polyamide system containing terminal NCO; 50g of allylamine was added to the viscous liquid, and the reaction was continued at 80℃ under nitrogen protection for 2h to obtain a viscous and transparent terminal ethylenically unsaturated polyamide. That is, the primary amine group was reacted with the terminal NCO, and then the cross-linking reaction of hydrogen-containing silicone oil with terminal ethylenically unsaturated polyamide and vinyl silicone rubber was used to obtain a silicone polyamide composite material with good waterproof performance and high temperature resistance.

[0018] Adipic acid: functionality is 2 (Hualu Hengsheng); polyetheramine, Mn=230, functionality is 2 (BASF); ethanolamine: amino functionality is 1 (Aladdin); diethanolamine: amino functionality is 1 (Aladdin); isocyanate ethyl acrylate: isocyanate functionality is 1 (Alpha Chemical); 4,4-dicyclohexylmethane diisocyanate (Wanhua Chemical)

[0071] DPHA: allylamine (Aladdin).

[0019] The remaining medicines are as follows: Vinyl silicone rubber is a polysiloxane with vinyl short links at both ends of the molecular chain. It is liquid and has a molecular weight of 15,000. The vinyl content is 0.015 to 0.02 mmol vinyl / g vinyl silicone rubber.

[0020] The hydrogen-containing silicone oil contains at least one polydimethyl silicone oil with Si-H bonds, and contains at least three silicon-hydrogen bonds on the molecular chain. The hydrogen content of the hydrogen-containing silicone oil is between 1.1 and 1.3 mmol / g.

[0021] The Pt catalyst is a Custer catalyst platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, which is a colorless to pale yellow liquid with a viscosity of 800 to 1000 mPa.s and a boiling point of 132 to 135°C. It can volatilize and leave the silicone tube system during high-temperature vulcanization.

[0022] The inhibitor is 1-ethynylcyclohexanol or vinylmethylcyclosiloxane, which is used to inhibit or delay the progress of the hydrosilation reaction.

[0023] Embodiment 1: A method for preparing a high temperature resistant glass fiber composite material, comprising the following steps: S1, Silicone Mix The terminal ethylenically unsaturated polyamide of Preparation Example 1, glass fiber, vinyl silicone rubber, hydrogenated silicone oil, Pt catalyst, and inhibitor were put into an internal mixer in a weight ratio of 100:30:20:2:0.8:0.002, and mixed for 30 minutes at a mixing temperature of 15-20° C.; S2, pre-crosslinking reaction 100:30-35:15-20:2-5:0.8-0.9:0.002-0.003 Increase the temperature of the internal mixer to 180-200°C, continue mixing for 30 minutes, stop stirring, and the system viscosity increases to 10000-12000cps; S3, Forming The mixed system obtained in S2 is put into an extrusion film-forming machine, the temperatures of zones 1-3 are 180°C, 210°C, and 250°C respectively, the outlet pressure is 10MPa, the cooling temperature is 20-30°C, and it is formed into a thin strip and curled to obtain a finished high-temperature resistant glass fiber composite material.

[0024] Example 2: Basically the same as Example 2, except that the weight ratio of terminal ethylenically unsaturated polyamide, glass fiber, vinyl silicone rubber, hydrogenated silicone oil, Pt catalyst and inhibitor is 100:32:18:4:0.85:0.0025.

[0025] Example 3: Basically the same as Example 3, except that the weight ratio of terminal ethylenically unsaturated polyamide, glass fiber, vinyl silicone rubber, hydrogenated silicone oil, Pt catalyst and inhibitor is 100:35:20:5:0.9:0.003.

[0026] Comparative Example 1: Polyamide PA66 and glass fiber were mixed in a weight ratio of 100:30 and prepared according to the conditions S3 in Example 1 to obtain a comparative product.

[0027] Performance Test: According to GB / T 8237-1987 "Liquid unsaturated polyester resin for glass fiber reinforced plastics (glass fiber reinforced plastics)", the performance tests were conducted on the finished high temperature resistant glass fiber composite materials (thickness 330 μm) obtained in Examples 1-3 and the product of Comparative Example 1, as shown in Table 1: Table 1. Comprehensive performance of finished high temperature resistant glass fiber composite materials

[0028] As can be seen from Table 1, as the silica gel content increases, the hydrophobicity and tensile strength are greatly improved, and the high temperature resistance and moisture resistance are better.

[0029] Example 4: The high-temperature resistant glass fiber composite product obtained by the preparation method described in Examples 1-3 is used in the preparation of FRP tanks. The high-temperature resistant glass fiber composite product is wound into a blank, and is subjected to high-temperature pressure holding and shaping at 250°C for 30 minutes, and then pressure holding and cooling to obtain a FRP tank.

[0030] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high temperature resistant glass fiber composite material, characterized in that: It includes the following components by weight: 100 parts of terminal ethylenically unsaturated polyamide, 30-35 parts of glass fiber, 15-20 parts of vinyl silicone rubber, 2-5 parts of hydrogen silicone oil, 0.8-0.9 parts of Pt catalyst, 0.002-0.003 inhibitor.

2. The high temperature resistant glass fiber composite material according to claim 1, characterized in that: The preparation process of the terminal olefinically unsaturated polyamide is as follows: 960 g of adipic acid and 1050 g of polyetheramine were placed in a reactor under a nitrogen atmosphere, and the reactor was heated to 170° C. until the amine value dropped below 0.1 mg / g, and 135 g of diethanolamine was first added dropwise using a dropping funnel to react for 1 hour, and then 200 g of ethanolamine was added dropwise; the mixture was then reacted at 170° C. for 3 hours, and the temperature was lowered to maintain 120° C. for dehydration for 30 minutes. After the dehydration was completed, the temperature was lowered to below 60° C., 400 g of ethyl isocyanate acrylate was added, and the temperature was raised to 80° C. to obtain a viscous liquid, thereby generating a polyamide system containing terminal NCO; 50 g of allylamine was added to the viscous liquid, and the reaction was continued at 80° C. under nitrogen protection for 2 hours to obtain a viscous and transparent terminal ethylenically unsaturated polyamide.

3. The high temperature resistant glass fiber composite material according to claim 1, characterized in that: The vinyl silicone rubber is a polysiloxane with vinyl short-circuits at both ends of the molecular chain, is in liquid form, has a molecular weight of 15,000, and a vinyl content of 0.015-0.02 mmol vinyl / g vinyl silicone rubber.

4. The high temperature resistant glass fiber composite material according to claim 1, characterized in that: The hydrogen-containing silicone oil contains at least one polydimethyl silicone oil with Si-H bonds, and contains at least 3 silicon-hydrogen bonds on the molecular chain. The hydrogen content of the hydrogen-containing silicone oil is between 1.1 and 1.3 mmol / g.

5. The high temperature resistant glass fiber composite material according to claim 1, characterized in that: The Pt catalyst is a Custer catalyst platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane, which is a colorless to pale yellow liquid with a viscosity of 800-1000 mPa.s and a boiling point of 132-135°C. It can volatilize and leave the silicone tube system during high-temperature vulcanization.

6. The high temperature resistant glass fiber composite material according to claim 1, characterized in that: The inhibitor is 1-ethynylcyclohexanol or vinylmethylcyclosiloxane, which is used to inhibit or delay the progress of the hydrosilation reaction.

7. The method for preparing a high temperature resistant glass fiber composite material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, Silicone Mix Put terminal ethylenically unsaturated polyamide, glass fiber, vinyl silicone rubber, hydrogenated silicone oil, Pt catalyst and inhibitor into an internal mixer according to a weight ratio of 100:30-35:15-20:2-5:0.8-0.9:0.002-0.003, and mix for 30 minutes at a mixing temperature of 15-20°C; S2. Pre-crosslinking reaction Increase the temperature of the internal mixer to 180-200°C, continue mixing for 30 minutes, stop stirring, and the system viscosity increases to 10000-12000cps; S3, Forming The mixed system obtained in S2 is put into an extrusion film-forming machine, the temperatures of zones 1-3 are 180°C, 210°C, and 250°C respectively, the outlet pressure is 10MPa, the cooling temperature is 20-30°C, and it is formed into a thin strip and curled to obtain a finished high-temperature resistant glass fiber composite material.

8. Use of the high temperature resistant glass fiber composite material product obtained by the preparation method of claim 7 in the preparation of glass fiber reinforced plastic tanks, winding the high temperature resistant glass fiber composite material product into a blank, subjecting it to high temperature pressure holding and shaping for 30 minutes at 250°C, and then cooling it under pressure to obtain a glass fiber reinforced plastic tank.

Citation Information

Patent Citations

  • A hydroxyl-terminated unsaturated polyamide, its preparation method and application

    CN111635521B

Cited By

  • Preparation method of bio-based nylon, antistatic bio-based nylon fabric as well as preparation method and application of antistatic bio-based nylon fabric

    CN121005895A