Environment-friendly two-component self-leveling floor material as well as preparation method and application thereof

Through the composite system of polydimethylsiloxane, epoxy resin and polyvinyl butyral, combined with environmentally friendly additives, the environmental protection and performance problems of traditional self-leveling materials are solved, and high-performance, environmentally friendly dual-dimensional products are developed. The components of self-leveling ground materials have achieved improvements in mechanical properties, flame retardant properties and construction convenience.

CN119081408AInactive Publication Date: 2024-12-06STATE GRID ANHUI ELECTRIC POWER CO LTD ELECTRIC POWER SCI RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411190014.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional self-leveling ground materials have many problems in environmental protection and performance, including harmful gas release of epoxy resin-based materials, poor dry shrinkage and cracking and impermeability of cement-based materials, high toxicity of polyurethane-based materials, and pure silicon The base material has insufficient mechanical strength and wear resistance.

Method used

Using a composite system of polydimethylsiloxane, epoxy resin and polyvinyl butyral, combined with environmentally friendly additives such as calcium lignin sulfonate and 4-aminophenyl disulfide, to optimize the component distribution ratio and process To form high-performance, environmentally friendly two-component self-leveling ground material.

Benefits of technology

It realizes the high mechanical properties, flame retardant properties, weather resistance and construction convenience of the material, reduces the environmental impact, meets increasingly stringent environmental protection requirements, and the overall performance exceeds the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081408A_ABST
    Figure CN119081408A_ABST
Patent Text Reader

Abstract

The invention discloses an environment-friendly two-component self-leveling floor material as well as a preparation method and application thereof, and belongs to the technical field of modified organic materials. The floor material is prepared from the following components in parts by weight: a component A: 43 to 52 parts of poly (dimethyl siloxane); 20 to 25 parts of epoxy resin; 4 to 8 parts of polyvinyl butyral; the component B comprises the following components in parts by weight: 0.2-0.6 part of calcium lignosulphonate; 0.1 part to 0.5 part of sorbitol ester; 2 to 5 parts of dioctyl phthalate; 5 to 10 parts of 4-aminophenyl disulfide; 1 to 3 parts of beta-glycerophosphoric acid; 2 to 7 parts of petroleum ether; and 0.5 to 2 parts of a modified stabilizer. The environment-friendly double-component self-leveling floor material developed by the invention realizes breakthrough in multiple aspects of environmental protection, mechanical property, weather resistance, constructability and the like, the overall performance comprehensively exceeds that of the prior art, and the environment-friendly double-component self-leveling floor material has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of modified organic materials, and in particular relates to an improved environmentally friendly two-component self-leveling floor material and a preparation method and application thereof. Background Art

[0002] As an indispensable part of modern construction and industry, self-leveling floor materials have received extensive attention and rapid development in recent years. This material has the advantages of automatic leveling, smooth surface, and easy construction, and has been widely used in industrial plants, commercial spaces, medical institutions and other places. However, with the improvement of environmental awareness and the deepening of the concept of sustainable development, the environmental problems and performance limitations faced by traditional self-leveling materials have become increasingly prominent, and new environmentally friendly materials are urgently needed to meet market demand.

[0003] Traditional self-leveling floor materials are mainly composed of epoxy resin, cement-based or polyurethane components. Although these materials have excellent performance in hardness, wear resistance and chemical stability, they also have many problems. First, epoxy resin-based materials will release harmful gases during the curing process, posing a potential threat to the health of construction workers and users. Secondly, although cement-based materials are environmentally friendly, they have defects such as shrinkage cracking and poor anti-seepage performance. Polyurethane-based materials do not meet increasingly stringent environmental protection requirements because the isocyanate raw materials used in their production process are highly toxic.

[0004] In recent years, researchers have begun to explore various new environmentally friendly materials to improve the performance of self-leveling floors. Silicon-based materials have attracted attention due to their excellent weather resistance, chemical stability and low toxicity. Polydimethylsiloxane (PDMS), as an important silicone polymer, has good flexibility, heat resistance and electrical insulation, and has broad application prospects in self-leveling materials. However, it is difficult to achieve the ideal mechanical strength and wear resistance by using PDMS alone, and it needs to be used in combination with other materials.

[0005] As the main component of traditional self-leveling materials, epoxy resin has excellent mechanical properties and bonding properties. However, it is brittle and easily turns yellow under ultraviolet light. Therefore, compounding epoxy resin with PDMS can improve the flexibility and weather resistance of the material while maintaining the excellent properties of epoxy resin. However, how to effectively compound the two materials and avoid phase separation is a major challenge facing researchers.

[0006] Polyvinyl butyral (PVB) is an excellent binder and toughening agent, and its application in composite materials is becoming more and more extensive. Introducing PVB into the PDMS / epoxy resin system is expected to further improve the mechanical properties and interfacial bonding of the material. However, the effect of the amount and dispersion of PVB on the final material properties needs further study.

[0007] In terms of environmentally friendly additives, calcium lignin sulfonate, as a byproduct of the papermaking industry, is low-cost and renewable. It can play a role in strengthening and toughening composite materials, and also has a certain flame retardant effect. However, the hydrophilicity of calcium lignin sulfonate is poorly compatible with organic matrices, and how to improve its dispersibility and interfacial bonding is an important issue.

[0008] Sorbitol ester surfactants, such as Span 20, can improve the compatibility and dispersibility of various components in composite materials. However, their dosage needs to be precisely controlled, as too much will affect the mechanical properties of the material. Dioctyl phthalate (DOP), as a commonly used plasticizer, can improve the flexibility and processing properties of materials, but its potential environmental hormone effect has attracted widespread attention, and more environmentally friendly alternatives need to be found.

[0009] 4-Aminophenyl disulfide is a new type of vulcanization accelerator and antioxidant, which is widely used in the rubber and plastics industries. Introducing it into self-leveling materials is expected to improve the anti-aging properties and thermal stability of the materials. However, its mechanism of action and optimal dosage in silicon-based materials need to be further studied.

[0010] As an organic phosphorus compound with good biocompatibility, β-glycerophosphate has been widely used in the field of biomaterials. Introducing it into self-leveling floor materials can not only improve the environmental friendliness of the materials, but also give the materials certain antibacterial properties. However, how to ensure the uniform dispersion and stability of β-glycerophosphate in the organic matrix is ​​a technical difficulty.

[0011] Petroleum ether is a commonly used organic solvent that can adjust the fluidity and curing speed of materials. However, its volatile organic compound (VOC) content is high and does not meet the increasingly stringent environmental protection requirements. Therefore, the development of low-VOC or VOC-free environmentally friendly solvent systems is an important direction for future research.

[0012] In summary, the development of new environmentally friendly two-component self-leveling floor materials faces many challenges and opportunities. How to reduce environmental impact and improve sustainability while ensuring material performance is the focus of future research. In addition, the compatibility, dispersibility and interface bonding between the components of the material, as well as the long-term performance and recyclability of the material, all require further in-depth research and exploration. Summary of the invention

[0013] In view of the problems existing in the above-mentioned prior art, the present invention provides an environmentally friendly two-component self-leveling floor material and its preparation method and application, adopts a composite system of polydimethylsiloxane, epoxy resin, and polyvinyl butyral, and utilizes the synergistic effect of the three to improve the mechanical properties and weather resistance of the material; adds environmentally friendly additives such as calcium lignin sulfonate and 4-aminophenyl disulfide to improve the material performance while reducing environmental impact; by optimizing the ratio of each component, the high performance and environmental friendliness of the material are achieved; the preparation method is simple, the components are mixed and stirred evenly in proportion, and then cast and solidified without complex equipment; the material can be widely used in floor coating in industrial plants, office buildings, warehouses and other places, and is particularly suitable for fields with high requirements for environmental protection and performance. The environmentally friendly two-component self-leveling floor material developed by the present invention has achieved breakthroughs in environmental protection, mechanical properties, weather resistance, construction performance and other aspects, and the overall performance comprehensively surpasses the existing technology, and has broad application prospects.

[0014] To solve the above problems, the present invention adopts the following technical solutions:

[0015] An environmentally friendly two-component self-leveling floor material, comprising the following components in parts by weight:

[0016] Component A:

[0017] Poly(dimethylsiloxane): 43 parts to 52 parts;

[0018] Epoxy resin: 20-25 parts;

[0019] Polyvinyl butyral: 4-8 parts;

[0020] Component B:

[0021] Calcium lignin sulfonate: 0.2-0.6 parts;

[0022] Sorbitol ester: 0.1-0.5 parts;

[0023] Dioctyl phthalate: 2-5 parts;

[0024] 4-aminophenyl disulfide: 5-10 parts;

[0025] β-glycerophosphate: 1-3 parts;

[0026] Petroleum ether: 2-7 parts;

[0027] Modified stabilizer: 0.5-2 parts;

[0028] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 40-60° C., and then the furfural solution is mixed with acrylic acid according to the mass ratio of furfural solution to acrylic acid (8-10): (2-3) and reacted at 80-85° C. for 3-4 hours.

[0029] Preferably, the environmentally friendly two-component self-leveling floor material,

[0030] In parts by weight, it includes the following components:

[0031] Component A:

[0032] Poly(dimethylsiloxane): 46-50 parts;

[0033] Epoxy resin: 22-25 parts;

[0034] Polyvinyl butyral: 4-8 parts;

[0035] Component B:

[0036] Calcium lignin sulfonate: 0.4-0.6 parts;

[0037] Sorbitol ester: 0.1-0.3 parts;

[0038] Dioctyl phthalate: 2-4 parts;

[0039] 4-aminophenyl disulfide: 5-7 parts;

[0040] β-glycerophosphate: 1-3 parts;

[0041] Petroleum ether: 2-5 parts;

[0042] Modified stabilizer: 0.5-2 parts;

[0043] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 40-60° C., and then the furfural solution is mixed with acrylic acid according to the mass ratio of furfural solution to acrylic acid (8-10): (2-3) and reacted at 80-85° C. for 3-4 hours.

[0044] Preferably, the environmentally friendly two-component self-leveling floor material,

[0045] In parts by weight, it includes the following components:

[0046] Component A:

[0047] Poly(dimethylsiloxane): 48 parts;

[0048] Epoxy resin: 24 parts;

[0049] Polyvinyl butyral: 6 parts;

[0050] Component B:

[0051] Calcium lignin sulfonate: 0.5 parts;

[0052] Sorbitol ester: 0.2 parts;

[0053] Dioctyl phthalate: 3 parts;

[0054] 4-aminophenyl disulfide: 6 parts;

[0055] β-Glycerol phosphate: 2 parts;

[0056] Petroleum ether: 4 parts;

[0057] Modified stabilizer: 1.5 parts;

[0058] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 50° C., and then the furfural solution is mixed with acrylic acid according to a mass ratio of furfural solution to acrylic acid of 9:2.5 and reacted at 83° C. for 3.5 hours.

[0059] The method for preparing the environmentally friendly two-component self-leveling floor material comprises the following steps:

[0060] Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid and petroleum ether are added to a poly(dimethylsiloxane) solution and stirred, and then epoxy resin, polyvinyl butyral and a modified stabilizer are added and uniformly mixed to form a prepolymer, which is cast into a finished product and cured at room temperature.

[0061] Preferably, the temperature of the poly(dimethylsiloxane) solution is 65°C-80°C.

[0062] Preferably, the mass concentration percentage of the poly(dimethylsiloxane) solution is 55%-70%.

[0063] Preferably, the stirring temperature is 90°C-110°C;

[0064] The stirring speed is 60rpm-120rpm;

[0065] The stirring time is 30min-50min.

[0066] Preferably, the uniform mixing method is mechanical stirring, the rotation speed is 120 rpm-180 rpm, and the temperature is 90°C-110°C.

[0067] Preferably, the prepolymer is formed by gradient cooling, the cooling rate is 1-5°C / min, and the temperature after cooling is 4°C;

[0068] The casting parameters are as follows: ambient humidity is 40%-60%, ambient temperature is 20°C;

[0069] The curing time is 24h-48h.

[0070] The modified stabilizer improves the fluidity and self-leveling properties of the floor material by interacting with poly(dimethylsiloxane) and epoxy resin. The addition of poly(dimethylsiloxane) helps to improve the wear resistance and crack resistance of the material.

[0071] The application of the environmentally friendly two-component self-leveling floor material as described above in the preparation of fireproof components.

[0072] At the same time, according to the patent application documents, the above-mentioned various raw materials mainly undergo the following reactions and interactions:

[0073] Polydimethylsiloxane (PDMS), epoxy resin and polyvinyl butyral (PVB) form an interpenetrating network structure. The hydroxyl groups in the PVB molecular chain can react chemically with the epoxy resin (the PVB molecular chain contains a large number of hydroxyl groups (-OH), which can react with the epoxy groups in the epoxy resin by ring-opening addition reaction. The -OH in PVB forms a hydrogen bond with the oxygen atom of the epoxy group. Under the action of the catalyst, the hydroxyl groups attack the epoxy ring, so that the ring-opening hydroxyl groups form a covalent bond with the carbon atom after the ring-opening, and at the same time generate new hydroxyl groups. This reaction process causes chemical cross-linking between PVB and the epoxy resin network), thereby improving the mechanical properties of the material. The active groups such as phenolic hydroxyl, carbonyl, and sulfonic acid groups in calcium lignin sulfonate can react chemically or physically interact with the matrix such as epoxy resin, thereby improving the interfacial bonding force between the filler and the matrix. Among them, the chemical reaction: a) Reaction of phenolic hydroxyl groups with epoxy groups: The phenolic hydroxyl groups in calcium lignin sulfonate can react with the epoxy groups of the epoxy resin by ring-opening addition reaction. This reaction will form new covalent bonds, chemically connecting calcium lignin sulfonate to the epoxy resin matrix and improving the interfacial bonding strength. The reaction equation is as follows: R-OH+CH 2 -CH-R′→RO-CH 2 -CH(OH)-R′R-OH+CH 2 -CH-R′→RO-CH 2 -CH(OH)-R′, where R represents the calcium lignin sulfonate molecule and R′ represents the epoxy resin molecule. b) Reaction of carbonyl group with epoxy group: The carbonyl group in calcium lignin sulfonate can also undergo addition reaction with epoxy group to form β-hydroxy ketone structure. This reaction also strengthens the chemical bonding between calcium lignin sulfonate and epoxy resin matrix. The reaction equation is as follows: RC=O+CH 2 -CH-R′-→RC(OH)-CH 2-CH(O)-R′RC=O+CH 2 -CH-R′→RC(OH)-CH 2 -CH(O)-R′. c) Catalytic effect of sulfonic acid group: Although sulfonic acid group does not directly participate in the chemical reaction, it can act as an acidic catalyst to promote the ring-opening polymerization reaction of epoxy resin and accelerate the curing process. Physical interaction: a) Hydrogen bonding: The phenolic hydroxyl, carbonyl and sulfonic acid groups in calcium lignin sulfonate can form hydrogen bonds with polar groups (such as hydroxyl, ether bonds, etc.) in epoxy resin molecules. This hydrogen bonding enhances the interfacial bonding between calcium lignin sulfonate and the matrix, and improves the mechanical properties of the composite material. b) Van der Waals force: There is a van der Waals force between calcium lignin sulfonate molecules and epoxy resin molecules. Although a single van der Waals force is weak, the cumulative effect of van der Waals forces between a large number of molecules can significantly enhance the interfacial bonding. c) Electrostatic interaction: The sulfonic acid group is negatively charged and can generate electrostatic attraction with the polar groups in the epoxy resin, further enhancing the interfacial bonding. When heated, calcium lignin sulfonate can also undergo intramolecular condensation and other reactions to form a cross-linked network structure. The amino group in the 4-aminophenyl disulfide molecule can react chemically with the epoxy resin to increase the crosslinking density of the material. Specifically, the reactive group: the amino group (-NH 2 ), epoxy resin molecules contain epoxy groups. Reaction type: This is a typical addition reaction between epoxy resin and amine compounds, which belongs to a ring-opening addition reaction. Reaction process: (1) The lone pair of electrons on the nitrogen atom in the amino group attacks the partially positively charged carbon atom in the epoxy group. (2) The epoxy ring opens, and the oxygen atom gains a proton to form a hydroxyl group. (3) The nitrogen atom forms a new covalent bond with the carbon atom. The reaction equation can be expressed as:

[0074]

[0075] Where R represents the benzene ring part of 4-aminophenyl disulfide, and R' represents the other parts of the epoxy resin molecule. 4-aminophenyl disulfide containing disulfide bonds can also undergo reversible exchange reactions, giving the material unique mechanical properties such as adaptability and stress relaxation. Sorbitol ester surfactants such as Span 20 can improve the compatibility and dispersibility of various components in composite materials, such as calcium lignin sulfonate fillers. β-glycerophosphate, as a flame retardant, can produce carbonization and release inert gas reactions when the material burns, thereby inhibiting the combustion of the material. Dioctyl phthalate (DOP) as a plasticizer can be inserted into the gaps between polymer molecular chains, increase the molecular chain spacing, and improve the flexibility of the material. Petroleum ether as a solvent can adjust the compatibility of various components, improve the fluidity of the material and the casting molding performance during the preparation process. In summary, in this environmentally friendly two-component self-leveling floor material, the components interact with each other through chemical reactions (such as condensation, addition reaction, etc.), physical interactions (such as hydrogen bonds, van der Waals forces, etc.), forming interpenetrating networks or cross-linked structures, etc., which jointly affect the mechanical properties, flame retardancy, process performance, etc. of the material. Reasonable optimization of the dosage of each component and reaction conditions can achieve synergistic efficiencies and obtain self-leveling floor materials with both high performance and environmentally friendly characteristics.

[0076] Compared with the prior art, the present invention has the following beneficial effects:

[0077] (1) Better environmental protection. The present invention adopts environmentally friendly materials such as polydimethylsiloxane and epoxy resin, and adds natural or low-toxic additives such as calcium lignin sulfonate and β-glycerophosphate. The overall formula is more environmentally friendly and has a low volatile organic compound (VOC) content, which meets the increasingly stringent environmental protection requirements.

[0078] (2) Excellent mechanical properties. Through reasonable design of the ratio, the self-leveling material of the present invention has excellent tensile strength (102.8-103.5MPa), elongation at break (234-246%) and other mechanical performance indicators, which are significantly better than the comparative example. The addition of epoxy resin and polyvinyl butyral plays a key role in improving strength and toughness.

[0079] (3) Outstanding flame retardant performance. After adding flame retardant additives such as p-glycerophosphoric acid, the limiting oxygen index of the material of the present invention can reach 32-37%, the flame retardant performance is greatly improved, and it is not easy to deform at high temperature.

[0080] (4) Good weather resistance and wear resistance. Polydimethylsiloxane is used as the matrix to give the material excellent weather resistance and wear resistance. Adding antioxidants such as 4-aminophenyl disulfide further improves aging resistance.

[0081] (5) Convenient construction and low cost. The self-leveling material of the present invention has excellent fluidity and self-leveling properties, high construction efficiency, and can quickly form a flat and smooth floor. The raw materials are easily available, the preparation method is simple, and the cost is low.

[0082] (6) Good decorative properties. Self-leveling materials can achieve a mirror-like smoothness and excellent decorative properties. Various pigments can be added to achieve a rich color selection.

[0083] In summary, the environmentally friendly two-component self-leveling floor material developed by the present invention has achieved breakthroughs in environmental protection, mechanical properties, flame retardancy, weather resistance, construction performance and other aspects. The overall performance comprehensively surpasses the existing technology and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0084] Figure 1 This is a physical picture of the environmentally friendly two-component self-leveling floor material prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0085] The present invention is further described below in conjunction with specific embodiments.

[0086] In the present invention, parts by weight are selected in kilograms (Kg) when used in specific applications.

[0087] The CAS numbers, manufacturers and other information of the chemical reagents used in the examples and comparative examples of the present invention are as follows:

[0088]

[0089] Example 1

[0090] Environmentally friendly two-component self-leveling floor material.

[0091] In parts by weight, it includes the following components:

[0092] Component A:

[0093] Poly(dimethylsiloxane): 43 parts;

[0094] Epoxy resin: 25 parts;

[0095] Polyvinyl butyral: 4 parts;

[0096] Component B:

[0097] Calcium lignin sulfonate: 0.2 parts;

[0098] Sorbitol ester: 0.5 part;

[0099] Dioctyl phthalate: 2 parts;

[0100] 4-aminophenyl disulfide: 10 parts;

[0101] β-Glycerol phosphate: 1 part;

[0102] Petroleum ether: 7 parts;

[0103] Modified stabilizer: 0.5 parts;

[0104] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 40° C., and then the furfural solution is mixed with acrylic acid at a mass ratio of 8:3 and reacted at 80° C. for 4 hours.

[0105] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0106] The parameters of poly(dimethylsiloxane) are as follows:

[0107] Density: 0.96g / cm 3 , viscosity: 800000cSt.

[0108] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0109] The parameters of epoxy resin are as follows:

[0110] Density: 1.4g / cm 3 , viscosity: 15000mPa·s.

[0111] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0112] The parameters of polyvinyl butyral are as follows:

[0113] Density: 1.08g / cm 3 , thermal decomposition temperature: 230℃.

[0114] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0115] The average particle size of calcium lignin sulfonate is 100 μm;

[0116] The sorbitol ester is Span 20, and its density is 1.05g / cm 3 ;

[0117] The viscosity of dioctyl phthalate is 9mPa·s and its density is 0.98g / cm 3 .

[0118] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0119] The appearance of 4-aminophenyl disulfide is light yellow crystalline powder;

[0120] The appearance of β-glycerophosphate is white crystalline powder;

[0121] The density of petroleum ether is 0.66 g / cm 3 .

[0122] A method for preparing an environmentally friendly two-component self-leveling floor material comprises the following steps:

[0123] Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid and petroleum ether are added to a poly(dimethylsiloxane) solution preheated to 65°C with a mass concentration of 70%, and stirred. The stirring temperature is 90°C, the stirring speed is 120rpm, and the stirring time is 30min. Then epoxy resin, polyvinyl butyral and modified stabilizer are added and evenly mixed. Mechanical stirring is adopted with a speed of 120rpm and a temperature of 110°C to form a prepolymer. The method is gradient cooling with a cooling rate of 1°C / min and a temperature of 4°C after cooling. The prepolymer is cast into a finished product. The casting environment humidity is 40% and the ambient temperature is 20°C. The product is cured at room temperature for 48h.

[0124] Example 2

[0125] Environmentally friendly two-component self-leveling floor material.

[0126] In parts by weight, it includes the following components:

[0127] Component A:

[0128] Poly(dimethylsiloxane): 52 parts;

[0129] Epoxy resin: 20 parts;

[0130] Polyvinyl butyral: 8 parts;

[0131] Component B:

[0132] Calcium lignin sulfonate: 0.6 parts;

[0133] Sorbitol ester: 0.1 part;

[0134] Dioctyl phthalate: 5 parts;

[0135] 4-aminophenyl disulfide: 5 parts;

[0136] β-Glycerol phosphate: 3 parts;

[0137] Petroleum ether: 2 parts;

[0138] Modified stabilizer: 2 parts;

[0139] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 60° C., and then the furfural solution is mixed with acrylic acid at a mass ratio of 10:2 and reacted at 85° C. for 3 hours.

[0140] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0141] The parameters of poly(dimethylsiloxane) are as follows:

[0142] Density: 0.96g / cm 3 , viscosity: 800000cSt.

[0143] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0144] The parameters of epoxy resin are as follows:

[0145] Density: 1.4g / cm 3 , viscosity: 15000mPa·s.

[0146] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0147] The parameters of polyvinyl butyral are as follows:

[0148] Density: 1.08g / cm 3 , thermal decomposition temperature: 230℃.

[0149] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0150] The average particle size of calcium lignin sulfonate is 100 μm;

[0151] The sorbitol ester is Span 20, and its density is 1.05g / cm 3 ;

[0152] The viscosity of dioctyl phthalate is 9mPa·s and its density is 0.98g / cm 3 .

[0153] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0154] The appearance of 4-aminophenyl disulfide is light yellow crystalline powder;

[0155] The appearance of β-glycerophosphate is white crystalline powder;

[0156] The density of petroleum ether is 0.66 g / cm 3 .

[0157] A method for preparing an environmentally friendly two-component self-leveling floor material comprises the following steps:

[0158] Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid and petroleum ether are added to a poly(dimethylsiloxane) solution preheated to 80°C with a mass concentration of 55%, and stirred. The stirring temperature is 110°C, the stirring speed is 60rpm, and the stirring time is 50min. Then epoxy resin, polyvinyl butyral and modified stabilizer are added and evenly mixed. Mechanical stirring is adopted with a speed of 180rpm and a temperature of 90°C to form a prepolymer. The method is gradient cooling with a cooling rate of 5°C / min and a temperature of 4°C after cooling. The prepolymer is cast into a finished product. The casting environment humidity is 60% and the ambient temperature is 20°C. The product is cured at room temperature for 24h.

[0159] Example 3

[0160] Environmentally friendly two-component self-leveling floor material.

[0161] In parts by weight, it includes the following components:

[0162] Component A:

[0163] Poly(dimethylsiloxane): 46 parts;

[0164] Epoxy resin: 25 parts;

[0165] Polyvinyl butyral: 4 parts;

[0166] Component B:

[0167] Calcium lignin sulfonate: 0.4 parts;

[0168] Sorbitol ester: 0.3 parts;

[0169] Dioctyl phthalate: 2 parts;

[0170] 4-aminophenyl disulfide: 7 parts;

[0171] β-Glycerol phosphate: 1 part;

[0172] Petroleum ether: 5 parts;

[0173] Modified stabilizer: 1 part;

[0174] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 45° C., and then the furfural solution is mixed with acrylic acid at a mass ratio of 8:2 and reacted at 80° C. for 3 hours.

[0175] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0176] The parameters of poly(dimethylsiloxane) are as follows:

[0177] Density: 0.96g / cm 3 , viscosity: 800000cSt.

[0178] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0179] The parameters of epoxy resin are as follows:

[0180] Density: 1.4g / cm 3 , viscosity: 15000mPa·s.

[0181] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0182] The parameters of polyvinyl butyral are as follows:

[0183] Density: 1.08g / cm 3 , thermal decomposition temperature: 230℃.

[0184] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0185] The average particle size of calcium lignin sulfonate is 100 μm;

[0186] The sorbitol ester is Span 20, and its density is 1.05g / cm 3 ;

[0187] The viscosity of dioctyl phthalate is 9mPa·s and its density is 0.98g / cm 3 .

[0188] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0189] The appearance of 4-aminophenyl disulfide is light yellow crystalline powder;

[0190] The appearance of β-glycerophosphate is white crystalline powder;

[0191] The density of petroleum ether is 0.66 g / cm 3 .

[0192] A method for preparing an environmentally friendly two-component self-leveling floor material comprises the following steps:

[0193] Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid and petroleum ether are added to a poly(dimethylsiloxane) solution preheated to 69°C with a mass concentration of 66%, and stirred at a temperature of 96°C, a speed of 110 rpm and a stirring time of 35 min. Then epoxy resin, polyvinyl butyral and modified stabilizer are added and uniformly mixed. Mechanical stirring is adopted at a speed of 130 rpm and a temperature of 95°C to form a prepolymer. The method is gradient cooling at a cooling rate of 2°C / min and a temperature after cooling of 4°C. The prepolymer is cast into a finished product. The casting environment humidity is 43% and the ambient temperature is 20°C. The product is cured at room temperature for 24 hours.

[0194] Example 4

[0195] Environmentally friendly two-component self-leveling floor material.

[0196] In parts by weight, it includes the following components:

[0197] Component A:

[0198] Poly(dimethylsiloxane): 50 parts;

[0199] Epoxy resin: 22 parts;

[0200] Polyvinyl butyral: 8 parts;

[0201] Component B:

[0202] Calcium lignin sulfonate: 0.6 parts;

[0203] Sorbitol ester: 0.1 part;

[0204] Dioctyl phthalate: 4 parts;

[0205] 4-aminophenyl disulfide: 5 parts;

[0206] β-Glycerol phosphate: 3 parts;

[0207] Petroleum ether: 2 parts;

[0208] Modified stabilizer: 1.5 parts;

[0209] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 60° C., and then the furfural solution is mixed with acrylic acid at a mass ratio of 10:3 and reacted at 85° C. for 4 hours.

[0210] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0211] The parameters of poly(dimethylsiloxane) are as follows:

[0212] Density: 0.96g / cm 3 , viscosity: 800000cSt.

[0213] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0214] The parameters of epoxy resin are as follows:

[0215] Density: 1.4g / cm 3 , viscosity: 15000mPa·s.

[0216] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0217] The parameters of polyvinyl butyral are as follows:

[0218] Density: 1.08g / cm 3 , thermal decomposition temperature: 230℃.

[0219] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0220] The average particle size of calcium lignin sulfonate is 100 μm;

[0221] The sorbitol ester is Span 20, and its density is 1.05g / cm 3 ;

[0222] The viscosity of dioctyl phthalate is 9mPa·s and its density is 0.98g / cm 3 .

[0223] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0224] The appearance of 4-aminophenyl disulfide is light yellow crystalline powder;

[0225] The appearance of β-glycerophosphate is white crystalline powder;

[0226] The density of petroleum ether is 0.66 g / cm 3 .

[0227] A method for preparing an environmentally friendly two-component self-leveling floor material comprises the following steps:

[0228] Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid and petroleum ether are added to a poly(dimethylsiloxane) solution preheated to 78°C with a mass concentration of 65%, and stirred. The stirring temperature is 105°C, the stirring speed is 80rpm, and the stirring time is 45min. Then epoxy resin, polyvinyl butyral and modified stabilizer are added and evenly mixed. Mechanical stirring is adopted with a speed of 170rpm and a temperature of 105°C to form a prepolymer. The method is gradient cooling with a cooling rate of 5°C / min and a temperature of 4°C after cooling. The prepolymer is cast into a finished product. The casting environment humidity is 55% and the ambient temperature is 20°C. The product is cured at room temperature for 48h.

[0229] Example 5

[0230] Environmentally friendly two-component self-leveling floor material.

[0231] In parts by weight, it includes the following components:

[0232] Component A:

[0233] Poly(dimethylsiloxane): 48 parts;

[0234] Epoxy resin: 24 parts;

[0235] Polyvinyl butyral: 6 parts;

[0236] Component B:

[0237] Calcium lignin sulfonate: 0.5 parts;

[0238] Sorbitol ester: 0.2 parts;

[0239] Dioctyl phthalate: 3 parts;

[0240] 4-aminophenyl disulfide: 6 parts;

[0241] β-Glycerol phosphate: 2 parts;

[0242] Petroleum ether: 4 parts;

[0243] Modified stabilizer: 1.5 parts;

[0244] The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 50° C., and then the furfural solution is mixed with acrylic acid according to a mass ratio of furfural solution to acrylic acid of 9:2.5 and reacted at 83° C. for 3.5 hours.

[0245] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0246] The parameters of poly(dimethylsiloxane) are as follows:

[0247] Density: 0.96g / cm 3 , viscosity: 800000cSt.

[0248] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0249] The parameters of epoxy resin are as follows:

[0250] Density: 1.4g / cm 3 , viscosity: 15000mPa·s.

[0251] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0252] The parameters of polyvinyl butyral are as follows:

[0253] Density: 1.08g / cm 3 , thermal decomposition temperature: 230℃.

[0254] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0255] The average particle size of calcium lignin sulfonate is 100 μm;

[0256] The sorbitol ester is Span 20, and its density is 1.05g / cm 3 ;

[0257] The viscosity of dioctyl phthalate is 9mPa·s and its density is 0.98g / cmm 3 .

[0258] The above-mentioned environmentally friendly two-component self-leveling floor material,

[0259] The appearance of 4-aminophenyl disulfide is light yellow crystalline powder;

[0260] The appearance of β-glycerophosphate is white crystalline powder;

[0261] The density of petroleum ether is 0.66 g / cm 3 .

[0262] A method for preparing an environmentally friendly two-component self-leveling floor material comprises the following steps:

[0263] Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid, and petroleum ether are added to a poly(dimethylsiloxane) solution preheated to 74°C with a mass concentration of 62%, and stirred. The stirring temperature is 100°C, the stirring speed is 80rpm, and the stirring time is 40min. Then epoxy resin, polyvinyl butyral and modified stabilizer are added and mixed evenly. Mechanical stirring is adopted with a speed of 150rpm and a temperature of 100°C to form a prepolymer. The method is gradient cooling with a cooling rate of 3°C / min. The temperature after cooling is 4°C. The prepolymer is cast into a finished product. The casting environment humidity is 40%-60%, and the ambient temperature is 20°C. It is cured at room temperature for 48h. Figure 1 , which is a picture of the cured product.

[0264] Comparative Example 1

[0265] The environmentally friendly two-component self-leveling floor material is based on Example 5, but differs in that the epoxy resin is removed.

[0266] Comparative Example 2

[0267] The environmentally friendly two-component self-leveling floor material is based on Example 5, but the difference is that polyvinyl acetal butyral is removed.

[0268] Comparative Example 3

[0269] The environmentally friendly two-component self-leveling floor material is based on Example 5, but differs in that calcium lignin sulfonate is removed.

[0270] Comparative Example 4

[0271] The environmentally friendly two-component self-leveling floor material is based on Example 5, but differs in that 4-aminophenyl disulfide is removed.

[0272] Comparative Example 5

[0273] The environmentally friendly two-component self-leveling floor material is based on Example 5, but differs in that: sodium β-glycerophosphate is removed.

[0274] Test Case

[0275] The floor materials prepared in Examples 1-5 and Comparative Examples 1-5 were selected and the following performance tests were performed:

[0276] Mechanical properties test: refer to GB / T 528-2009, use electronic universal material testing machine for testing, tensile rate 50mm / main, test temperature 25℃. Sample size is set to 50mm×4mm×2mm. Measure three times and take the average value.

[0277] Flame retardant performance test:

[0278] According to the method specified in GB / T 2406.2-2009, the sample size was set to 150 mm × 10 mm × 10 mm; the oxygen index of the sample was measured using an HC-2CZ oxygen index tester.

[0279] High temperature resistance, low temperature resistance and thermal insulation performance testing:

[0280] The sample size was set to 150 mm × 10 mm × 10 mm, and the changes were tested at 250°C and -40°C. The thermal insulation performance was determined by testing the thermal conductivity.

[0281] Table 1 Test results of Examples 1-5

[0282]

[0283] As shown in Table 1, the test results of Examples 1-5 show that the main properties are as follows: tensile strength: 102.8-103.5MPa, elongation at break: 234-246%, oxygen index: 32-37%, high and low temperature resistance: no deformation at 250℃ / -40℃, thermal conductivity: 0.04-0.06W / (m·K). Innovation: A composite system of poly(dimethylsiloxane), epoxy resin and polyvinyl butyral is used, and environmentally friendly additives such as calcium lignin sulfonate and 4-aminophenyl disulfide are added. By optimizing the distribution ratio of each component, excellent mechanical properties, flame retardancy and temperature resistance are achieved. In general, the invention has developed a self-leveling floor material with comprehensive performance and environmental friendliness through reasonable design of formula and process, which has good application prospects.

[0284] Table 2 Comparative Examples 1-5 Test Results

[0285]

[0286] From Table 2, the epoxy resin is removed in Comparative Example 1. According to the formula of Comparative Example 1, after removing the epoxy resin, the performance of the composite material has changed significantly, and the tensile strength and elongation at break have dropped significantly. The mechanism is analyzed as follows: Epoxy resin is the matrix of the composite material, which plays a role in bonding the components into a whole. After removing the epoxy resin, the material loses the matrix, the internal structure is loose, and the mechanical properties are greatly reduced. Epoxy resin has excellent mechanical properties, such as high strength, high modulus, good wear resistance, etc. After removing the epoxy resin, the material loses the contribution of this high-performance component, resulting in a decrease in mechanical properties such as tensile strength. Epoxy resin has good compatibility with other components such as polydimethylsiloxane (PDMS), polyvinyl butyral (PVB), etc., and can form an interpenetrating network structure to improve the mechanical properties of the material. Removing the epoxy resin destroys the interpenetrating network structure of the material, causing the performance to decline. Epoxy resin participates in the formation of the chemical cross-linked network structure of the material. After removing the epoxy resin, the cross-linking density decreases, and the strength and toughness of the material decrease. Epoxy resin has excellent bonding properties and can firmly bond inorganic fillers to organic matrices. When epoxy resin is removed, the interfacial bonding force between the filler and the matrix decreases, and the mechanical properties of the material decrease. In summary, as a key matrix component of composite materials, epoxy resin plays a vital role in maintaining material integrity, providing mechanical properties, forming an interpenetrating network structure, participating in chemical cross-linking, and bonding fillers. When epoxy resin is removed, the microstructure and properties of the composite material undergo fundamental changes, resulting in a significant decrease in key mechanical performance indicators such as tensile strength and elongation at break. Therefore, when designing environmentally friendly composite materials, the presence and amount of epoxy resin are crucial, and it is necessary to optimize while taking into account both environmental protection and material properties.

[0287] In Comparative Example 2, polyvinyl butyral is removed. According to the formula of Comparative Example 2, after polyvinyl butyral (PVB) is removed, the tensile strength and elongation at break of the composite material are both reduced. The mechanism is analyzed as follows: PVB is an excellent binder and toughening agent, which plays a role of toughening and bonding in polymer-based composite materials. After removing PVB, the bonding force between the components inside the material decreases, the interface bonding force deteriorates, and the mechanical properties decrease. The PVB molecular chain contains a large number of hydroxyl groups, which can react chemically with thermosetting resins such as epoxy resin to form an interpenetrating network structure and improve the mechanical properties of the material. Removing PVB destroys this interpenetrating network structure, which reduces the strength and toughness of the material. PVB has excellent film-forming properties and toughness, and the formed coating has high transparency, high elasticity and impact resistance. Removing PVB, the material loses the contribution of this tough component, and the elongation at break decreases. PVB can improve the rheological properties of the matrix such as epoxy resin and improve the processing properties of the composite material. Removing PVB, the fluidity of the material deteriorates, the processing properties decrease, resulting in defects inside the material, thereby affecting the mechanical properties. PVB has a good dispersing effect on inorganic fillers such as calcium lignin sulfonate. After removing PVB, the dispersibility of the filler becomes worse, and it is easy to agglomerate in the matrix, forming stress concentration, resulting in a decrease in mechanical properties. In summary, PVB, as an excellent binder and toughening agent, plays an important role in maintaining the integrity of composite materials, improving interfacial bonding, forming an interpenetrating network structure, giving materials toughness, and dispersing fillers. After removing PVB, the microstructure of the composite material and the interaction between the components change, ultimately leading to a decrease in mechanical properties such as tensile strength and elongation at break. Therefore, when designing environmentally friendly composite materials, the presence and amount of PVB need to be considered comprehensively, taking into account the mechanical properties of the material while meeting environmental protection requirements.

[0288] Calcium lignin sulfonate is removed in Comparative Example 3. According to the formula of Comparative Example 3, after calcium lignin sulfonate is removed, the tensile strength and elongation at break of the composite material are both reduced. The mechanism is analyzed as follows: Calcium lignin sulfonate, as a natural polymer filler, plays a role of reinforcement and filling in the composite material. After calcium lignin sulfonate is removed, the material loses the contribution of this reinforcing component and the mechanical properties are reduced. Calcium lignin sulfonate molecules contain a large number of active groups such as phenolic hydroxyl, carbonyl, and sulfonic acid groups, which can react chemically or physically with matrices such as epoxy resins to improve the interfacial bonding force between the filler and the matrix. After calcium lignin sulfonate is removed, the interfacial bonding force between the filler and the matrix decreases, resulting in poor mechanical properties. Calcium lignin sulfonate has excellent dispersibility and can be evenly dispersed in the polymer matrix to play a role in transferring stress. After calcium lignin sulfonate is removed, the dispersibility of the filler deteriorates, and it is easy to agglomerate in the matrix, forming stress concentration, which ultimately leads to poor mechanical properties. Calcium lignin sulfonate can undergo intramolecular condensation and other reactions when heated to form a cross-linked network structure, thereby improving the thermal stability and mechanical properties of the material. When calcium lignin sulfonate is removed, the material loses the contribution of this thermosetting group. Calcium lignin sulfonate can act as a nucleating agent to induce crystallization of the polymer matrix, thereby improving crystallinity and mechanical properties. When calcium lignin sulfonate is removed, the crystallization behavior of the material is affected, the crystallinity decreases, and the mechanical properties deteriorate. In summary, as a natural polymer filler with excellent performance, calcium lignin sulfonate plays multiple roles in environmentally friendly composite materials, such as reinforcement, filling, coupling, and nucleation. After calcium lignin sulfonate is removed, the composite material loses these beneficial effects, and the microstructure and mechanical properties change, ultimately leading to a decrease in tensile strength and elongation at break. Therefore, the rational use of calcium lignin sulfonate and the optimization of its dosage and dispersion state in composite materials are of great significance for the development of high-performance environmentally friendly materials.

[0289] 4-aminophenyl disulfide is removed in Comparative Example 4. According to the formula of Comparative Example 4, after removing 4-aminophenyl disulfide, the tensile strength and elongation at break of the composite material are both reduced, but the high temperature and low temperature resistance performance is deformed. The mechanism is analyzed as follows: 4-aminophenyl disulfide contains disulfide bonds and can be used as a key component of self-repairing materials. Removing this component, the material loses its self-repairing function and is difficult to repair itself when damaged by external forces, resulting in a decrease in mechanical properties. 4-aminophenyl disulfide molecules contain amino groups, which can react chemically with epoxy resin to increase the cross-linking density of the material. Removing this component, the cross-linking density decreases, and the strength and toughness of the material decrease. Disulfide bonds can undergo reversible exchange reactions, giving the material unique mechanical properties such as adaptability and stress relaxation. Removing components containing disulfide bonds, the material loses these special properties. 4-aminophenyl disulfide can also be used as a rubber vulcanization accelerator to improve the mechanical properties of the rubber matrix. It plays a similar role in this system, and removal leads to a decrease in the mechanical properties of the matrix. Compounds containing disulfide bonds have certain antioxidant properties and can improve the aging resistance of the material. Removing this component leads to a decrease in the heat resistance of the material and easy deformation at high temperatures. In summary, 4-aminophenyl disulfide, as a key component containing disulfide bonds, can improve the mechanical properties and heat resistance of composite materials through various mechanisms such as self-repair, chemical reaction, and dynamic cross-linking. After removing this component, the material loses its self-repair ability, the cross-linking density decreases, the mechanical properties decrease, and the heat resistance deteriorates, and it is easy to deform at high temperatures. Therefore, the presence of 4-aminophenyl disulfide is crucial to maintaining the comprehensive performance of the material. When designing environmentally friendly self-healing materials, its dosage can be appropriately reduced, but complete removal will lead to a significant decrease in performance.

[0290] The removal of β-glycerophosphate in comparative example 5 affects the performance of the environmentally friendly two-component self-leveling floor material in the following way: β-glycerophosphate, as an organic phosphorus compound, mainly plays a flame retardant role in composite materials. Removing β-glycerophosphate will reduce the flame retardant properties of the material. β-glycerophosphate can be used as a serine-threonine phosphatase inhibitor in the kinase reaction buffer. Removing this component will affect the conduction of certain enzymatic reactions in the material. β-glycerophosphate can be used as a phosphate donor to promote the differentiation of mesenchymal stem cells into osteoblasts in cell culture medium. Removing this component will affect the biocompatibility of the material and its ability to induce osteogenic differentiation. In the chitosan / β-sodium glycerophosphate (CS / β-GP) thermosensitive hydrogel system, β-sodium glycerophosphate can stabilize the chitosan solution under neutral conditions and give the material thermosensitive properties. Removing β-sodium glycerophosphate will destroy the thermosensitive hydrogel structure. β-Sodium glycerophosphate can accelerate the calcification of cultured vascular smooth muscle cells through alkaline phosphatase-related mechanisms. Removing this component will reduce the ability of the material to induce calcification deposition. In summary, β-glycerophosphate affects the performance of environmentally friendly two-component self-leveling floor materials mainly through mechanisms such as flame retardancy, enzyme reaction regulation, induction of cell differentiation, construction of thermosensitive hydrogels, and promotion of calcification. Removing β-glycerophosphate will reduce the flame retardancy, biocompatibility, thermosensitivity and other properties of the material, but the impact on mechanical properties is relatively small. In practical applications, the amount of β-glycerophosphate needs to be comprehensively considered to meet the material performance requirements while taking into account environmental protection and cost factors.

[0291] The above content is a further detailed description of the present invention in combination with specific implementation methods. It cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the scope of protection determined by the claims submitted for the present invention.

Claims

1. An environmentally friendly two-component self-leveling floor material, characterized by: In parts by weight, it includes the following components: Component A: Poly(dimethylsiloxane): 43 parts to 52 parts; Epoxy resin: 20-25 parts; Polyvinyl butyral: 4-8 parts; Component B: Calcium lignin sulfonate: 0.2-0.6 parts; Sorbitol ester: 0.1-0.5 parts; Dioctyl phthalate: 2-5 parts; 4-aminophenyl disulfide: 5-10 parts; β-glycerophosphate: 1-3 parts; Petroleum ether: 2-7 parts; Modified stabilizer: 0.5-2 parts; The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 40-60° C., and then the furfural solution is mixed with acrylic acid according to the mass ratio of furfural solution to acrylic acid (8-10): (2-3) and reacted at 80-85° C. for 3-4 hours.

2. The environmentally friendly two-component self-leveling floor material according to claim 1, characterized in that: In parts by weight, it includes the following components: Component A: Poly(dimethylsiloxane): 46-50 parts; Epoxy resin: 22-25 parts; Polyvinyl butyral: 4-8 parts; Component B: Calcium lignin sulfonate: 0.4-0.6 parts; Sorbitol ester: 0.1-0.3 parts; Dioctyl phthalate: 2-4 parts; 4-aminophenyl disulfide: 5-7 parts; β-glycerophosphate: 1-3 parts; Petroleum ether: 2-5 parts; Modified stabilizer: 0.5-2 parts; The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 40-60°C, and then the furfural solution is mixed with acrylic acid according to the mass ratio of furfural solution to acrylic acid (8-10): (2-3) and reacted at 80-85°C for 3-4h.

3. The environmentally friendly two-component self-leveling floor material according to claim 2, characterized in that: In parts by weight, it includes the following components: Component A: Poly(dimethylsiloxane): 48 parts; Epoxy resin: 24 parts; Polyvinyl butyral: 6 parts; Component B: Calcium lignin sulfonate: 0.5 parts; Sorbitol ester: 0.2 parts; Dioctyl phthalate: 3 parts; 4-aminophenyl disulfide: 6 parts; β-Glycerol phosphate: 2 parts; Petroleum ether: 4 parts; Modified stabilizer: 1.5 parts; The preparation method of the modified stabilizer is as follows: 60 mg / L furfural solution is mixed in a stirrer at 50° C., and then the furfural solution is mixed with acrylic acid according to a mass ratio of furfural solution to acrylic acid of 9:2.5 and reacted at 83° C. for 3.5 hours.

4. The method for preparing the environmentally friendly two-component self-leveling floor material according to any one of claims 1 to 3, characterized in that: The steps include: Calcium lignin sulfonate, sorbitol ester, dioctyl phthalate, 4-aminophenyl disulfide, β-glycerophosphoric acid and petroleum ether are added to a poly(dimethylsiloxane) solution and stirred, and then epoxy resin, polyvinyl butyral and a modified stabilizer are added and uniformly mixed to form a prepolymer, which is cast into a finished product and cured at room temperature.

5. The method for preparing the environmentally friendly two-component self-leveling floor material according to claim 4, characterized in that: The temperature of the poly(dimethylsiloxane) solution is 65°C-80°C.

6. The method for preparing the environmentally friendly two-component self-leveling floor material according to claim 5, characterized in that: The mass concentration percentage of the poly(dimethylsiloxane) solution is 55%-70%.

7. The method for preparing the environmentally friendly two-component self-leveling floor material according to claim 6, characterized in that: The stirring temperature is 90°C-110°C; The stirring speed is 60rpm-120rpm; The stirring time is 30min-50min.

8. The method for preparing the environmentally friendly two-component self-leveling floor material according to claim 7, characterized in that: The uniform mixing method is mechanical stirring, the rotation speed is 120rpm-180rpm, and the temperature is 90℃-110℃.

9. The method for preparing the environmentally friendly two-component self-leveling floor material according to claim 8, characterized in that: The method of forming the prepolymer is gradient cooling, the cooling rate is 1-5°C / min, and the temperature after cooling is 4°C; The casting parameters are as follows: ambient humidity is 40%-60%, ambient temperature is 20°C; The curing time is 24h-48h.

10. Use of the environmentally friendly two-component self-leveling floor material according to any one of claims 1 to 3 in the preparation of fireproof parts.