Compatible and stable waste plastic recycled asphalt material and preparation method thereof
By using composite solubilizers and antioxidants in modified asphalt, the compatibility and stability of waste plastics and asphalt are improved, the problem of poor storage stability of waste plastics modified asphalt is solved, and more efficient resource reuse and Performance improvement.
Patent Information
- Application Number
- CN202411348189.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the storage stability of waste plastic modified asphalt is poor, and improper solubilizer selection leads to poor modification effect, making it difficult to make full use of waste plastic resources.
The composition of composite modified asphalt, including matrix asphalt, plastic, composite solubilizer and antioxidant, is combined with appropriate antioxidants to enhance the plastic by combining polyphosphoric acid, dioctyl maleate, aromatic oil and other composite solubilizers. Compatibility and stability with asphalt.
It significantly improves the low-temperature performance and storage stability of modified asphalt, reduces the accumulation of plastic waste in the environment, reduces the demand for raw materials, and has good environmental and economic benefits.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering and environmental protection, and specifically relates to a waste plastic modified asphalt and a modified asphalt mixture and a preparation method thereof. Background Art
[0002] With the rapid development of the global economy and the accelerated advancement of urbanization, the amount of waste plastics has increased dramatically, posing a huge challenge to environmental protection and resource recycling. The treatment and recycling of waste plastics has become one of the focuses of global attention. Traditional methods for the treatment of waste plastics include incineration, landfill and mechanical recycling, but these methods have problems such as environmental pollution, waste of resources and energy consumption.
[0003] In order to effectively solve the problem of waste plastic treatment and resource recycling, many researchers and companies are committed to developing new recycling technologies. Among them, using waste plastics as modifiers in the preparation of asphalt mixtures has become a method that has attracted much attention. This method can not only achieve the recycling of waste plastic resources, but also improve the performance of asphalt mixtures, and improve their anti-aging, durability and environmental adaptability.
[0004] At present, the main methods for preparing modified asphalt are dry method and wet method. However, the dry method has problems such as uneven mixing, poor adhesion, and poor performance improvement, making it difficult to fully utilize waste plastic resources. For example, in the patent "A kind of waste thermosetting plastic modified asphalt and modified asphalt mixture" (patent application number: CN201410838543.0), by processing waste thermosetting plastics into a particle size similar to that of mineral powder, fine aggregate, etc., it partially replaces mineral powder, fine aggregate and asphalt. Although the high temperature performance and strength of asphalt and asphalt mixture are improved, there is still the problem that waste plastics cannot be evenly dispersed in asphalt, resulting in poor modification effect.
[0005] In contrast, wet modification has greater potential, but it also faces challenges. Wet modification can disperse waste plastics more evenly in the asphalt matrix, significantly improving the high temperature performance and low temperature flexibility of asphalt. However, the poor compatibility between waste plastics and asphalt leads to poor storage stability of the modified asphalt. For example, the patent "A Method for Preparing Waste Plastic Modified Asphalt" (patent application number: CN201611068091.8) has improved on the traditional preparation method and improved the high temperature performance and low temperature flexibility of asphalt through the wet method, but the prepared asphalt still has the disadvantage of poor storage stability.
[0006] In order to solve the problem of poor storage stability of waste plastic modified asphalt, researchers have tried to add solubilizers to improve the compatibility between plastic and asphalt, thereby improving the storage stability of modified asphalt. However, there are many types of solubilizers currently used, and the most suitable solubilizer has not been selected for a specific plastic, resulting in poor improvement in the storage stability of modified asphalt. Therefore, it is necessary to study and solve the problem of poor compatibility between waste plastics and asphalt from multiple aspects (melt index, solubilizer, matrix asphalt) to promote the application of waste plastics in the field of road engineering materials. Summary of the invention
[0007] In order to solve at least one of the above problems, the present invention provides a composite modified asphalt, characterized in that the components include: base asphalt, plastic, composite solubilizer, antioxidant,
[0008] in,
[0009] The composite solubilizer is composited from polyphosphoric acid and at least one of dioctyl maleate, aromatic oil and epoxidized soybean oil.
[0010] The inventors have explored the various components of the composite modified asphalt. For base asphalts with different penetrations, selecting waste plastics with suitable particle sizes and solubility parameters can better improve the asphalt performance, and for different waste plastics, selecting suitable antioxidants can better improve the asphalt performance. At the same time, the selection of solubilizers is also one of the important factors. In the prior art, there are many types of solubilizers, but only a specific combination of solubilizers can better improve the asphalt performance. Even the same type of solubilizers play different roles in the same combination.
[0011] According to a specific embodiment of the present invention, the mass ratio of the base asphalt, plastic, composite solubilizer and antioxidant is (80-120): (1-7): (1-15): (0.08-1.5).
[0012] According to a specific embodiment of the present invention, the components of the composite modified asphalt include, by mass, 80-120 parts of base asphalt, 1-7 parts of plastic, 1-15 parts of composite solubilizer, and 0.08-1.5 parts of antioxidant.
[0013] According to a specific embodiment of the present invention, the plastic includes polar plastic and non-polar plastic.
[0014] According to a specific embodiment of the present invention, the polar plastic includes polyethylene terephthalate, polyurethane, and polyvinyl chloride.
[0015] According to a specific embodiment of the present invention, the non-polar plastic includes polyethylene and polypropylene.
[0016] According to a specific embodiment of the present invention, the melt index of the plastic is (10-20) g / 10 min.
[0017] According to a specific embodiment of the present invention, the particle size of the plastic is 200-400 meshes.
[0018] According to a specific embodiment of the present invention, the base asphalt has a needle penetration grade of 70 or 90.
[0019] According to a specific embodiment of the present invention, when the solubility parameter difference between the plastic and the asphalt is greater than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90.
[0020] According to a specific embodiment of the present invention, when the solubility parameter difference between the plastic and asphalt is less than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90 or 70.
[0021] According to a specific embodiment of the present invention, the antioxidant includes a thioester antioxidant and an aromatic amine antioxidant.
[0022] According to a specific embodiment of the present invention, the thioester antioxidant includes lauryl thiodipropionate, octadecyl thiodipropionate and 3-lauryl thiopropionate.
[0023] According to a specific embodiment of the present invention, the aromatic amine antioxidant includes dioctyl diphenylamine, dinonyl diphenylamine, and butyl octyl diphenylamine.
[0024] According to a specific embodiment of the present invention, when the plastic is a polar plastic, the antioxidant is a thioester antioxidant.
[0025] According to a specific embodiment of the present invention, when the plastic is a non-polar plastic, the antioxidant is an aromatic amine antioxidant.
[0026] According to a specific embodiment of the present invention, in the composite solubilizing agent, the mass ratio of the polyphosphoric acid to at least one of the dioctyl maleate, aromatic oil, and epoxidized soybean oil is 1:(4-9).
[0027] According to a specific embodiment of the present invention, the aromatic oil is furfural extracted oil.
[0028] A second aspect of the present invention provides a method for preparing a composite modified asphalt, comprising:
[0029] S1. Pre-treating the plastic to obtain plastic particles with a particle size of 200-400 mesh;
[0030] S2, adding the pretreated plastic into the molten matrix asphalt, stirring and swelling;
[0031] S3, adding solubilizing agent 1 to the base asphalt after stirring and swelling in step S2, and performing high-speed shearing;
[0032] S4, adding the solubilizer 2 and the antioxidant to the base asphalt after high-speed shearing in step S3 to obtain the composite modified asphalt,
[0033] in,
[0034] The solubilizer 1 includes polyphosphoric acid, and the solubilizer 2 includes at least one of dioctyl maleate, aromatic oil, and epoxidized soybean oil.
[0035] According to a specific embodiment of the present invention, the mass ratio of the solubilizer 1 to the solubilizer 2 is 1:(4-9).
[0036] According to a specific embodiment of the present invention, in the solubilizing agent 2, the aromatic oil is furfural extracted oil.
[0037] According to a specific embodiment of the present invention, the solubilizer 1 and the solubilizer 2 are a composite solubilizer, and in the composite modified asphalt, the mass ratio of the base asphalt, plastic, composite solubilizer and antioxidant is (80-120): (1-7): (1-15): (0.08-1.5).
[0038] According to a specific embodiment of the present invention, the plastic includes polar plastic and non-polar plastic.
[0039] According to a specific embodiment of the present invention, the polar plastic includes polyethylene terephthalate, polyurethane, and polyvinyl chloride.
[0040] According to a specific embodiment of the present invention, the non-polar plastic includes polyethylene and polypropylene.
[0041] According to a specific embodiment of the present invention, the melt index of the plastic is (10-20) g / 10 min.
[0042] According to a specific embodiment of the present invention, the base asphalt has a needle penetration grade of 70 or 90.
[0043] According to a specific embodiment of the present invention, when the solubility parameter difference between the plastic and the asphalt is greater than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90.
[0044] According to a specific embodiment of the present invention, when the solubility parameter difference between the plastic and asphalt is less than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90 or 70.
[0045] According to a specific embodiment of the present invention, the antioxidant includes a thioester antioxidant and an aromatic amine antioxidant.
[0046] According to a specific embodiment of the present invention, the thioester antioxidant includes lauryl thiodipropionate, octadecyl thiodipropionate and 3-lauryl thiopropionate.
[0047] According to a specific embodiment of the present invention, the aromatic amine antioxidant includes dioctyl diphenylamine, dinonyl diphenylamine, and butyl octyl diphenylamine.
[0048] According to a specific embodiment of the present invention, when the plastic is a polar plastic, the antioxidant is a thioester antioxidant.
[0049] According to a specific embodiment of the present invention, when the plastic is a non-polar plastic, the antioxidant is an aromatic amine antioxidant.
[0050] The stable waste plastic recycled asphalt material of the present invention has the beneficial effect of improving the low-temperature performance and storage stability of the modified asphalt compared with the prior art: the present invention fully mixes waste plastics with specific properties with asphalt with specific needle penetration through wet modification, adds an appropriate proportion of specific composite solubilizers to the modified asphalt, and selects specific antioxidants so that the plastic can be fully and evenly dissolved in the asphalt, thereby further improving the storage stability of the waste plastic modified asphalt. The method of the present invention has good environmental and economic benefits: using waste plastics for asphalt modification effectively reduces the accumulation of plastic waste in the environment and reduces plastic pollution; using waste plastics as modifiers can reduce the demand for some raw materials, thereby reducing costs. DETAILED DESCRIPTION
[0051] The embodiments of the present invention are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0052] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.
[0053] In this document, the terms “contain”, “include” or “comprise” are open expressions, that is, they include the contents specified in the present invention but do not exclude other contents.
[0054] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.
[0055] In this article, the term "needle penetration" refers to the depth of a standard cone (usually with a total load of 150 grams, and sometimes 100 grams) that sinks into a grease sample kept at 25°C within 5 seconds. The unit is 1 / 10 mm. The greater the needle penetration, the softer the grease, that is, the smaller the viscosity; conversely, the harder the grease, that is, the greater the viscosity. For the determination of the needle penetration of asphalt, a standard sharp needle with a total load of 100 grams is used instead of a standard cone. The measurement conditions are the same as those for grease.
[0056] In this article, the term "plastic" refers to a material that has resin (or monomers directly polymerized during processing) as the main component, and additives such as plasticizers, fillers, lubricants, and colorants as auxiliary components, and can flow and form during processing. Plastics are synthetic polymer compounds that can change their shapes freely. Plastics are materials that are polymerized by synthesis or condensation reactions using monomer raw materials. They are composed of synthetic resins and additives such as fillers, plasticizers, stabilizers, lubricants, and colorants. Its main component is synthetic resin.
[0057] In this article, the term "base asphalt" refers to the base asphalt used to produce modified asphalt, which is modified by adding asphalt modifiers.
[0058] In this article, the term "thermoplastic" refers to plastics that soften when heated and harden when cooled. Most of the plastics used in daily life belong to this category. When heated, it softens and even flows, and when cooled, it hardens. This process is reversible and can be repeated. Polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, acrylic plastics, other polyolefins and their copolymers, polysulfones, polyphenylene ether, chlorinated polyether, etc. are all thermoplastics. The resin molecular chains in thermoplastics are all linear or branched structures. There are no chemical bonds between the molecular chains. When heated, they soften and flow. The process of cooling and hardening is a physical change. Thermoplastics belong to thermoplastic polymer materials.
[0059] As used herein, the term "thermoplastic polymer material" refers to a polymer material that softens when heated and hardens when cooled.
[0060] In this article, the term "high-density polyethylene" (HDPE) is a white powder or granular product. It is non-toxic, odorless, with a crystallinity of 80% to 90%, a softening point of 125 to 135°C, and an operating temperature of up to 100°C; its hardness, tensile strength and creep are better than those of low-density polyethylene; its wear resistance, electrical insulation, toughness and cold resistance are better; its chemical stability is good, and it is insoluble in any organic solvent at room temperature, and is resistant to corrosion by acids, alkalis and various salts; its film has low permeability to water vapor and air, and low water absorption; its aging resistance is poor, and its resistance to environmental stress cracking is not as good as that of low-density polyethylene, especially thermal oxidation will reduce its performance, so antioxidants and ultraviolet absorbers must be added to the resin to improve this aspect. The heat deformation temperature of high-density polyethylene film is low under stress, so you should pay attention to it when using it.
[0061] In this article, the term "low-density polyethylene" refers to waxy white, tasteless, odorless, non-toxic, matte waxy granules with a density range of 0.910-0.925 g / cms. It is the lightest variety of polyethylene resin except ultra-low-density polyethylene. Its molecular structure is a branched molecule with long and short branches on the main chain, with about 20-30 ethyl, butyl or longer branches per 1,000 carbon atoms on the main chain. Compared with high-density polyethylene and medium-density polyethylene, it has lower crystallinity (55%-65%) and softening point (90-100°C), and a wider melt flow rate (MFI = 0.2-80 g / min).
[0062] As used herein, the term "furfural-extracted oil" refers to the undesirable components of lubricating oil separated by dissolving in the furfural solvent after vacuum distillate oil or solvent deasphalted oil is extracted with a furfural solvent.
[0063] In this article, the term "epoxidized soybean oil" (ESO) is a type of organic substance with a chemical formula of (RC2H2OR'COO)3C3H5. It is a light yellow viscous oily liquid at room temperature. It is non-toxic. The boiling point is 150℃ (0.53kPa). It is soluble in most organic solvents and hydrocarbons, but insoluble in water.
[0064] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, by referring to these contents, ordinary technicians in the field should be able to understand other possible implementation methods and advantages of the present invention.
[0065] The present invention proposes a compatible and stable waste plastic recycled asphalt material and a preparation method thereof. The storage stability of waste plastic modified asphalt can be improved, and the low temperature performance of waste plastic modified asphalt can be improved. The material is made of a mixture of base asphalt, waste plastic, composite solubilizer and antioxidant, and based on 100 parts by weight of the base asphalt, 1-7 parts by weight of the waste plastic, 5-20 parts by weight of the composite solubilizer and 0.1-1 part of the antioxidant.
[0066] The waste plastics selected in the present invention are divided into polar plastics and non-polar plastics, among which non-polar plastics are preferably high-density polyethylene, low-density polyethylene and polypropylene; polar plastics are preferably polyethylene terephthalate, polyurethane and polyvinyl chloride. Since the density of plastics has a great influence on the asphalt modification effect, the higher the density of plastics, the higher the melting point and thermal stability, which easily leads to local agglomeration or accumulation of plastic particles in asphalt; but when the density of plastics is low, it also increases the risk of stratification and phase separation of waste plastic modified asphalt, thereby affecting the storage stability of modified asphalt. After exploration, the present invention selects waste plastics with a density range of 0.90-1.35g / cm 3 .
[0067] In addition to the great influence of the density and crystallinity of plastics on the modification effect of asphalt, the melt index of plastics also has a great influence on the compatibility of asphalt after modification. The melt index of plastics reflects the fluidity of plastics under high temperature conditions. When the melt index is too high, the plastic has better fluidity and dispersibility when mixed with asphalt, but it will also lead to a decrease in high temperature performance; when the melt index is too low, after the asphalt is modified, it has better high temperature stability and strength, but its fluidity is low, and the dispersibility of plastics in asphalt is poor. When the melt index of waste plastics screened by the present invention is in the range of 10 to 20 g / 10 min, the modified asphalt can have excellent stability, strength and dispersibility.
[0068] The compounding of the composite solubilizer is composed of at least one of polyphosphoric acid and dioctyl maleate, aromatic oil, and epoxidized soybean oil, and its composite mass ratio is 1:4~9. The selected polyphosphoric acid can dissolve the asphaltene in the asphalt, so that the waste plastic is dispersed more evenly in the asphalt, and the storage stability of the modified asphalt is improved, but the low temperature performance of the modified asphalt is also reduced. The selected dioctyl maleate, epoxidized soybean oil and aromatic oil have strong dissolving power, which can be used as a surfactant, not only can effectively dissolve plastics, but also improve the swelling ability of asphalt to waste plastics, thereby improving the storage stability between plastics and asphalt, and also improving the low temperature performance of waste plastic modified asphalt, so polyphosphoric acid is compounded with it, while improving the storage stability of asphalt, it also improves the low temperature performance of asphalt after polyphosphoric acid is added. At the same time, the inventor has found through a lot of exploration that not all aromatic oils are suitable for the present invention, and the aldehyde extracted oil screened out by the present invention has a better improvement effect on waste plastic modified asphalt relative to other aromatic solubilizers.
[0069] In addition to the control of plastic materials and solubilizers, the type of base asphalt also affects the performance of asphalt modified from waste plastics. Asphalt with a penetration grade of 90 has more aromatic hydrocarbon components than asphalt with a penetration grade of 70. Therefore, when the crystallinity of the plastic is high or the solubility parameters differ greatly, it is easier to select asphalt with a high penetration grade so that the plastic can be fully dispersed in the asphalt. Therefore, the selection method of the base asphalt of the present invention is set as follows: the solubility parameter difference with the asphalt is greater than 10 (J / cm3) 0.5 , preferably asphalt with a penetration grade of 90; the difference in solubility parameters of waste plastics is less than 10 (J / cm3) 0.5 , choose asphalt with a needle penetration grade of 90 or asphalt with a needle penetration grade of 70.
[0070] The inventors of the present application have screened out specific antioxidants according to the different types of waste plastic modifiers to fully improve the anti-aging properties of modified asphalt. Since polar plastics and thioester antioxidants have good compatibility, polar antioxidants should be given priority. This type of antioxidant usually contains functional groups that can interact with polar groups, such as hydroxyl groups, amino groups, etc., thereby improving the antioxidant properties of modified asphalt; aromatic amine antioxidants can effectively inhibit the oxidation reaction in asphalt and non-polar plastic modified asphalt, reduce the generation and accumulation of free radicals, thereby improving the antioxidant properties and stability of modified asphalt, and can also delay the phase separation process by reducing the occurrence of oxidation reactions, thereby indirectly improving the stability of the blending system. Therefore, the scheme of the present invention is: if the selected plastic is a polar plastic, a thioester antioxidant is selected, among which lauryl thiodipropionate, octadecyl thiodipropionate and 3-lauryl thiopropionate are preferred; if the selected plastic is a non-polar plastic, an aromatic amine antioxidant is selected, among which dioctyl diphenylamine, dinonyl diphenylamine and butyl octyl diphenylamine are preferred.
[0071] In a second aspect, the present invention also provides a method for preparing a compatible and stable modified waste plastic recycled asphalt material, the specific steps of which are as follows:
[0072] S1, pre-treating the waste plastics, granulating, crushing, cleaning and drying the waste plastics, and then grinding the dried waste plastics with a grinding wheel to a particle size of 300 meshes for later use;
[0073] S2. Place the selected base asphalt in an oven at 160-170°C to completely melt the base asphalt;
[0074] S3, putting the completely melted matrix asphalt into a uniform speed stirrer, slowly adding the waste plastic powder obtained in step S1 into the matrix asphalt, stirring for 30 minutes at 180°C and 1000rpm to make it fully swell;
[0075] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add the composite solubilizer, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0076] S5. Put the fully mixed asphalt into a uniform speed mixer, slowly add antioxidant to the asphalt at 170° C. and a rotation speed of 1000 rpm, stir for 30 minutes, and finally obtain waste plastic modified asphalt.
[0077] The main reagents and reagent acquisition sources involved in the present invention are shown in Table 1.
[0078] Table 1
[0079]
[0080] It should be noted that the reagents and consumables involved in the present invention can be obtained through conventional purchase, and the asphalts of different penetration degrees of the present invention can also be obtained by those skilled in the art through conventional means. The technical scheme in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] Example 1
[0082] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 12 g of high-density polyethylene (MFI: 15 g / 10 min), 40 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 0.4 g of dioctyl diphenylamine.
[0083] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0084] S1. Pre-treat the waste high-density polyethylene plastic by granulating, crushing, cleaning and drying it, and then grind the dried high-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh, and then use it for standby.
[0085] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0086] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 12 g of the high-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0087] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0088] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% by mass of furfural extracted oil, then add 0.4g of 0.1% by mass of dioctyldiphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0089] Example 2
[0090] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 12 g of high-density polyethylene (MFI: 10 g / 10 min), 40 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 0.4 g of dioctyl diphenylamine.
[0091] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0092] S1. Pre-treat the waste high-density polyethylene plastic by granulating, crushing, cleaning and drying it, and then grind the dried high-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh, and then use it for standby.
[0093] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0094] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 12 g of the high-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0095] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0096] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% by mass of furfural extracted oil, then add 0.4g of 0.1% by mass of dioctyldiphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0097] Example 3
[0098] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 12 g of high-density polyethylene (MFI: 20 g / 10 min), 40 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 0.4 g of dioctyl diphenylamine.
[0099] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0100] S1. Pre-treat the waste high-density polyethylene plastic by granulating, crushing, cleaning and drying it, and then grind the dried high-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh, and then use it for standby.
[0101] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0102] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 12 g of the high-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0103] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0104] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% by mass of furfural extracted oil, then add 0.4g of 0.1% by mass of dioctyldiphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0105] Example 4
[0106] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400g of 90# asphalt, 20g of low-density polyethylene (MFI: 15g / 10min), 24g of composite solubilizer (mass ratio: polyphosphoric acid: dioctyl maleate = 1:5), and 2g of butyl octyl diphenylamine.
[0107] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0108] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0109] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0110] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0111] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0112] S5. Put the fully mixed asphalt into a uniform speed mixer, add 20g of dioctyl maleate with a mass fraction of 5%, and then add 2g of butyl octyl diphenylamine with a mass fraction of 0.5%, stir for 30 minutes at 170°C and a rotation speed of 1000rpm, and finally obtain waste plastic modified asphalt.
[0113] Example 5
[0114] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 24 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 2 g of butyl octyl diphenylamine.
[0115] This embodiment also provides a method for preparing compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0116] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0117] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0118] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0119] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0120] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% furfural extracted oil by mass, then add 2g of 0.5% butyl octyl diphenylamine by mass, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0121] Example 6
[0122] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 24 g of composite solubilizer (mass ratio: polyphosphoric acid: epoxy soybean oil = 1:5), and 2 g of butyl octyl diphenylamine.
[0123] This embodiment also provides a method for preparing compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0124] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0125] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0126] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0127] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0128] S5. Put the fully mixed asphalt into a uniform speed mixer, add 20g of 5% epoxy soybean oil, then add 2g of 0.5% butyl octyl diphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0129] Comparative Example 1
[0130] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 12 g of high-density polyethylene (MFI: 5 g / 10 min), 40 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 0.4 g of dioctyl diphenylamine.
[0131] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0132] S1, pre-treating the waste high-density polyethylene, granulating, crushing, cleaning and drying it, and then grinding the dried high-density polyethylene with a grinding wheel to a particle size of 300 mesh for standby use;
[0133] S2, put 400g of asphalt with a needle penetration grade of 90 into an oven at 160°C and completely melt it;
[0134] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 12 g of the high-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0135] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0136] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% by mass of furfural extracted oil, then add 0.4g of 0.1% by mass of dioctyldiphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0137] Comparative Example 2
[0138] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 12 g of high-density polyethylene (MFI: 50 g / 10 min), 40 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 0.4 g of dioctyl diphenylamine.
[0139] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0140] S1. Pre-treat the waste high-density polyethylene plastic by granulating, crushing, cleaning and drying it, and then grind the dried high-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh, and then use it for standby.
[0141] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0142] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 12 g of the high-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0143] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0144] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% by mass of furfural extracted oil, then add 0.4g of 0.1% by mass of dioctyldiphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0145] Comparative Example 3
[0146] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 70# asphalt, 12 g of high-density polyethylene (MFI: 15 g / 10 min), 40 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:9), and 0.4 g of dioctyl diphenylamine.
[0147] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0148] S1, pre-treating the waste high-density polyethylene, granulating, crushing, cleaning and drying it, and then grinding the dried high-density polyethylene with a grinding wheel to a particle size of 300 mesh for standby use;
[0149] S2. Place 400 g of asphalt with a penetration grade of 70 into an oven at 160° C. and completely melt it;
[0150] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 12 g of the high-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0151] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0152] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% by mass of furfural extracted oil, then add 0.4g of 0.1% by mass of dioctyldiphenylamine, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0153] Comparative Example 4
[0154] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400g of 90# asphalt, 20g of low-density polyethylene (MFI: 15g / 10min), 24g of composite solubilizer (mass ratio: polyphosphoric acid: dioctyl phthalate = 1:5), and 2g of butyl octyl diphenylamine.
[0155] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0156] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to 300 mesh for standby use;
[0157] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0158] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20 g of the low-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0159] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0160] S5. Put the fully mixed asphalt into a uniform speed mixer, add 20g of dioctyl phthalate with a mass fraction of 5%, and then add 2g of butyl octyl diphenylamine with a mass fraction of 0.5%, stir for 30 minutes at 170°C and a rotation speed of 1000rpm, and finally obtain waste plastic modified asphalt.
[0161] Comparative Example 5
[0162] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 4 g of polyphosphoric acid, and 2 g of butyl octyl diphenylamine.
[0163] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0164] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to 300 mesh for standby use;
[0165] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0166] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20 g of the low-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0167] S4. Put the swollen asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1%, and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0168] S5. Put the fully mixed asphalt into a uniform speed mixer, add 2 g of 0.5% by mass of butyl octyl diphenylamine, stir for 30 minutes at 170° C. and a rotation speed of 1000 rpm, and finally obtain waste plastic modified asphalt.
[0169] Comparative Example 6
[0170] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 20 g of dioctyl maleate, and 2 g of butyl octyl diphenylamine.
[0171] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0172] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to 300 mesh for standby use;
[0173] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0174] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20 g of the low-density polyethylene powder obtained in step S1 into the asphalt, stirring at 180° C. and 1000 rpm for 30 min to fully swell it;
[0175] S4. Put the swollen asphalt into a high-speed shear emulsifier and perform high-speed shearing for 30 minutes at 180°C and 6000rpm.
[0176] S5. Put the fully mixed asphalt into a uniform speed mixer, add 20g of dioctyl maleate with a mass fraction of 5%, and then add 2g of butyl octyl diphenylamine with a mass fraction of 0.5%, stir for 30 minutes at 170°C and a rotation speed of 1000rpm, and finally obtain waste plastic modified asphalt.
[0177] Comparative Example 7
[0178] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 24 g of composite solubilizer (mass ratio: polyphosphoric acid: rubber oil = 1:9), and 2 g of butyl octyl diphenylamine.
[0179] This embodiment also provides a method for preparing a compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0180] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0181] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0182] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0183] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0184] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of rubber oil with a mass fraction of 9%, and then add 2g of butyl octyl diphenylamine with a mass fraction of 0.5%, stir for 30 minutes at 170°C and a rotation speed of 1000rpm, and finally obtain waste plastic modified asphalt.
[0185] Comparative Example 8
[0186] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 24 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:3), and 2 g of butyl octyl diphenylamine.
[0187] This embodiment also provides a method for preparing compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0188] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0189] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0190] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0191] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0192] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% furfural extracted oil by mass, then add 2g of 0.5% butyl octyl diphenylamine by mass, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0193] Comparative Example 9
[0194] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400 g of 90# asphalt, 20 g of low-density polyethylene (MFI: 15 g / 10 min), 24 g of composite solubilizer (mass ratio: polyphosphoric acid: furfural extracted oil = 1:12), and 2 g of butyl octyl diphenylamine.
[0195] This embodiment also provides a method for preparing compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0196] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0197] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0198] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0199] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0200] S5. Put the fully mixed asphalt into a uniform speed mixer, add 36g of 9% furfural extracted oil by mass, then add 2g of 0.5% butyl octyl diphenylamine by mass, stir for 30min at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0201] Comparative Example 10
[0202] The present embodiment provides a compatible and stable waste plastic modified asphalt material, including the following components: 400g of 90# asphalt, 20g of low-density polyethylene (MFI: 15g / 10min), 24g of composite solubilizer (mass ratio: polyphosphoric acid: epoxidized linseed oil = 1:5), and 2g of butyl octyl diphenylamine.
[0203] This embodiment also provides a method for preparing compatible and stable waste plastic modified asphalt, and the preparation method is as follows:
[0204] S1, pre-treating the waste low-density polyethylene plastic, granulating, crushing, cleaning and drying it, and then grinding the dried low-density polyethylene plastic with a grinding wheel to a particle size of 300 mesh for standby use;
[0205] S2. Put 400 g of asphalt with a penetration grade of 90 into an oven at 160° C. and melt it completely;
[0206] S3, putting the completely melted asphalt into a uniform speed stirrer, slowly adding 20g of the low-density polyethylene plastic powder obtained in step S1 into the asphalt, stirring for 30min at 180°C and 1000rpm to fully swell it;
[0207] S4. Put the swollen base asphalt into a high-speed shear emulsifier, add 4g of polyphosphoric acid with a mass fraction of 1% at 180°C and 6000rpm, and perform high-speed shearing for 30 minutes.
[0208] S5. Put the fully mixed asphalt into a uniform speed mixer, add 20g of 9% epoxidized linseed oil, then add 2g of 0.5% butyl octyl diphenylamine, stir for 30 minutes at 170°C and 1000rpm, and finally obtain waste plastic modified asphalt.
[0209] In order to verify the relevant properties of waste plastic modified asphalt materials, physical property tests were carried out according to the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTJE20-2011), and the physical properties of the modified asphalt in the examples were analyzed; polymer modified asphalt segregation tests were carried out according to the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTJE20-2011), and the storage stability of the modified asphalt in the examples was analyzed, as shown in Table 2:
[0210] Table 2 Softening point, low temperature ductility and segregation test results
[0211]
[0212]
[0213] As shown in Table 2, by comparing Examples 1 to 3 with Comparative Examples 1 to 3, it can be seen that the plastic modified asphalt with a plastic melt index within 10 to 20 g / 10 min has better storage stability than the plastic modified asphalt with a melt index of 5 g / 10 min and 50 g / 10 min. Although the plastic modified asphalt with a plastic melt index of 5 g / 10 min has good storage stability, its high temperature performance is poor; although the melt index of 50 g / 10 min has good high temperature performance, its storage stability is poor. By comparing Example 1 with Comparative Example 3, it can be concluded that when the crystallinity of the plastic is high or the solubility parameter is greatly different from that of the asphalt, asphalt with a higher penetration grade is selected as the base asphalt because it contains more aromatic components, and the modified asphalt obtained has better storage stability. By comparing the test results of Example 4 with those of Comparative Example 4, dioctyl maleate is selected as one of the composite solubilizers, which has a better improvement effect on the low-temperature ductility and storage stability of the modified asphalt; the solubilizers used in Comparative Examples 5 and 6 are single solubilizers, and the incorporation of a single solubilizer, polyphosphoric acid, has a low-temperature ductility that is significantly lower than that of Example 4 and Comparative Example 6, and the incorporation of a single solubilizer, dioctyl maleate, has a softening point that is lower than that of Example 4 and Comparative Example 5; due to the addition of polyphosphoric acid, the high-temperature performance of the asphalt is enhanced, but the low-temperature toughness of the asphalt is also weakened. Through the composite modification with dioctyl maleate, the modification effects of the two solubilizers on the asphalt are complementary, which not only enhances the high-temperature performance of the modified asphalt, but also improves the low-temperature toughness of the modified asphalt. It can be concluded from the separation test results that the incorporation of the composite solubilizer significantly reduces the softening point difference compared to the incorporation of a single solubilizer, indicating that the composite solubilizer has a better effect on improving the storage stability of the modified asphalt. By comparing Example 5 with Comparative Example 7, the softening point and low-temperature ductility of Example 5 are higher than those of Comparative Example 7, and the softening point difference of Example 5 is smaller than that of Comparative Example 7. Therefore, the furfural extracted oil in the composite solubilizer has a better improvement effect on waste plastic modified asphalt than other aromatic solubilizers. By comparing Example 5 with Comparative Example 8 and Comparative Example 9, when the component ratio of the composite compatibilizer is small, its softening point does not change, but its low-temperature performance and storage stability are poor; when the component ratio of the composite solubilizer is high, due to the increase in the content of furfural extracted oil, its low-temperature performance and storage stability are poor, but its high-temperature performance decreases. By comparing Example 6 with Comparative Example 10, epoxidized soybean oil is relative to epoxidized linseed oil. When it is added to waste plastic modified asphalt, the high-temperature performance and low-temperature performance of asphalt are more obvious, and the softening point difference is also reduced, which improves the storage stability of waste plastic modified asphalt.
[0214] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite modified asphalt, characterized in that: The ingredients include: Base asphalt, plastic, composite solubilizer, antioxidant, in, The composite solubilizer is composited from polyphosphoric acid and at least one of dioctyl maleate, aromatic oil and epoxidized soybean oil.
2. The composite modified asphalt according to claim 1, characterized in that: The mass ratio of the matrix asphalt, plastic, composite solubilizer and antioxidant is (80-120): (1-7): (1-15): (0.08-1.5); The components of the composite modified asphalt include, by weight, 80-120 parts of base asphalt, 1-7 parts of plastic, 1-15 parts of composite solubilizer, and 0.08-1.5 parts of antioxidant.
3. The composite modified asphalt according to claim 1, characterized in that: The plastics include polar plastics and non-polar plastics; The polar plastics include polyethylene terephthalate, polyurethane, and polyvinyl chloride; The non-polar plastics include polyethylene and polypropylene.
4. The composite modified asphalt according to claim 1, characterized in that: The melt index of the plastic is (10-20) g / 10min; The particle size of the plastic is 200-400 meshes.
5. The composite modified asphalt according to claim 1, characterized in that: The base asphalt has a needle penetration grade of 70 or 90; When the solubility parameter difference between the plastic and asphalt is greater than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90; When the solubility parameter difference between the plastic and asphalt is less than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90 or 70.
6. The composite modified asphalt according to claim 1, characterized in that: The antioxidants include thioester antioxidants and aromatic amine antioxidants; The thioester antioxidants include lauryl thiodipropionate, octadecyl thiodipropionate and 3-lauryl thiopropionate; The aromatic amine antioxidants include dioctyl diphenylamine, dinonyl diphenylamine and butyl octyl diphenylamine.
7. The composite modified asphalt according to claim 1, characterized in that: When the plastic is a polar plastic, the antioxidant is a thioester antioxidant; When the plastic is a non-polar plastic, the antioxidant is an aromatic amine antioxidant.
8. The composite modified asphalt according to claim 1, characterized in that: In the composite solubilizer, the mass ratio of the polyphosphoric acid to at least one of the dioctyl maleate, aromatic oil, and epoxidized soybean oil is 1:(4-9); The aromatic oil is furfural extracted oil.
9. A method for preparing composite modified asphalt, characterized in that: include: S1. Pre-treating the plastic to obtain plastic particles with a particle size of 200-400 mesh; S2, adding the pretreated plastic into the molten matrix asphalt, stirring and swelling; S3, adding solubilizing agent 1 to the base asphalt after stirring and swelling in step S2, and performing high-speed shearing; S4, adding the solubilizer 2 and the antioxidant to the base asphalt after high-speed shearing in step S3 to obtain the composite modified asphalt, in, The solubilizer 1 includes polyphosphoric acid, and the solubilizer 2 includes at least one of dioctyl maleate, aromatic oil, and epoxidized soybean oil.
10. The method according to claim 9, characterized in that The mass ratio of the solubilizer 1 to the solubilizer 2 is 1:(4-9); In the solubilizing agent 2, the aromatic oil is furfural extracted oil; The solubilizer 1 and the solubilizer 2 are a composite solubilizer. In the composite modified asphalt, the mass ratio of the base asphalt, the plastic, the composite solubilizer and the antioxidant is (80-120): (1-7): (1-15): (0.08-1.5); The plastics include polar plastics and non-polar plastics; The polar plastics include polyethylene terephthalate, polyurethane, and polyvinyl chloride; The non-polar plastics include polyethylene and polypropylene; The melt index of the plastic is (10-20) g / 10min; The base asphalt has a needle penetration grade of 70 or 90; When the solubility parameter difference between the plastic and asphalt is greater than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90; When the solubility parameter difference between the plastic and asphalt is less than 10 (J / cm 3 ) 0.5 When the base asphalt has a needle penetration grade of 90 or 70; The antioxidants include thioester antioxidants and aromatic amine antioxidants; The thioester antioxidants include lauryl thiodipropionate, octadecyl thiodipropionate and 3-lauryl thiopropionate; The aromatic amine antioxidants include dioctyl diphenylamine, dinonyl diphenylamine, and butyl octyl diphenylamine; When the plastic is a polar plastic, the antioxidant is a thioester antioxidant; When the plastic is a non-polar plastic, the antioxidant is an aromatic amine antioxidant.
Citation Information
Cited By
Asphalt modifier, method for modifying asphalt through cooperation of organic montmorillonite, waste plastic and nucleating agent, and modified asphalt
CN122011546A