Green low-temperature-resistant composite asphalt material as well as preparation method and application thereof
The green low-temperature composite asphalt material prepared by using raw materials such as rock asphalt, lignin sulfonate modified asphalt, waste ceramic particles and oyster shell modified rubber particles has solved the crack resistance of existing asphalt pavement materials in low temperature environments. The problem of insufficient performance has achieved good mechanical properties and crack resistance in severe cold areas, while alleviating the pressure of solid waste treatment.
Patent Information
- Application Number
- CN202411494351.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-12-06
AI Technical Summary
The existing asphalt pavement materials have insufficient crack resistance in low temperature environments, especially when used in severe cold areas, and traditional methods have great pressure on solid waste treatment.
A green low-temperature composite asphalt material is prepared by using raw materials such as rock asphalt, lignin sulfonate modified asphalt, waste ceramic particles and oyster shell modified rubber particles. It is modified by palm oil and modified rubber particles by palm fiber modified by palm oil. Improve the toughness and crack resistance of the material, and use steel slag micro powder to enhance strength.
It significantly improves the rut and crack resistance of asphalt materials at low temperatures, reduces temperature sensitivity, and uses natural and solid waste materials to achieve economical and environmentally friendly road surface material solutions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of highway pavement materials, and in particular to a green low-temperature resistant composite asphalt material and a preparation method and application thereof. Background Art
[0002] Asphalt pavement is a common pavement structure that is continuous, seamless, high-strength, comfortable to drive, low-noise, and easy to maintain, and is increasingly favored by highway builders. The performance of common petroleum asphalt is generally insufficient to bear heavy traffic, which causes increasingly serious damage to the pavement, mainly manifested in rutting, oil spills, and bulges caused by insufficient high-temperature stability, and shrinkage cracks caused by insufficient low-temperature crack resistance that affect driving safety. In order to solve these problems, engineers have proposed a variety of solutions.
[0003] Natural rock asphalt is a material composed of an inorganic mixture and an asphalt matrix, usually formed in rock cracks. After being processed into powder, natural rock asphalt has good compatibility with ordinary matrix asphalt, which can increase the viscosity and elasticity of asphalt mixtures. Rock asphalt can also improve the high temperature performance, anti-aging performance and water stability of asphalt mixtures, effectively improving the road performance of petroleum asphalt.
[0004] However, it has been found through actual use that although the addition of rock asphalt can improve the high-temperature stability and anti-aging properties of asphalt pavement to a certain extent, it will have a certain impact on the low-temperature crack resistance of asphalt mixture. In the existing technology, the low-temperature performance of rock asphalt is mostly improved by adding rubber powder, but the effect is still difficult to meet the use needs in cold areas. Therefore, the development of a green and environmentally friendly asphalt mixture with excellent low-temperature resistance is of great practical significance for the development of highway pavement materials. Summary of the invention
[0005] In view of the problem that the asphalt pavement with rock asphalt as the main raw material in the prior art has poor low temperature resistance, the present invention provides a green low temperature resistant composite asphalt material and its preparation method and application. The present invention uses rock asphalt, lignin sulfonate modified asphalt, waste ceramic particles and oyster shell modified rubber particles as raw materials to prepare a green low temperature resistant composite asphalt material with wear resistance and excellent mechanical properties. The green low temperature resistant composite asphalt material has simple ingredients and a simple preparation process, and uses waste ceramics and waste rubber as raw materials, which greatly alleviates the processing pressure of these two wastes and provides a more economical and environmentally friendly technical solution for highway pavement materials.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The first aspect of the present invention provides a green low-temperature resistant composite asphalt material, comprising the following raw material components in percentage by weight: 5%-30% rock asphalt, 25%-40% base asphalt, 3%-5% palm oil modified SBS resin, 5%-10% steel slag powder and 20%-30% palm fiber modified rubber particles.
[0007] Compared with the prior art, the present invention uses rock asphalt, a natural asphalt component, and matrix asphalt as the main asphalt components. Since the nitrogen element in rock asphalt exists in the form of functional groups, the strong wettability and high resistance to natural oxidants of the composite asphalt material are improved, thereby improving the anti-aging performance of the composite asphalt material. And since rock asphalt is a natural asphalt material, it is stable in nature and has good weather resistance. It can be well compatible with matrix asphalt, reduce the temperature sensitivity of the composite asphalt material, enhance its toughness and crack resistance in low temperature environments, and improve the anti-rutting ability of the composite asphalt material at low temperatures. The addition of palm oil-modified SBS resin can form a large number of cross-linked structures, and then supplemented by the filling of steel slag powder, improve the strength and low-temperature cracking resistance of the composite asphalt material.
[0008] The present invention also adds palm fiber modified rubber particles to the composite asphalt material. The rubber modified by palm fiber has a three-dimensional network structure, which greatly improves the toughness of the asphalt material, realizes the coating of the asphalt component and the steel slag powder seasoning, and improves the compactness between the components, thereby improving the cohesion and temperature stability of the composite asphalt material. Even in cold areas, the composite asphalt material can maintain good mechanical properties and crack resistance. More importantly, the raw materials of the present invention are mostly from natural materials and solid waste materials. While maintaining good performance, it effectively alleviates the processing pressure of solid waste materials, develops the use performance of natural rock asphalt, and conforms to the concept of green building material development.
[0009] Preferably, the preparation method of the palm oil modified SBS resin comprises the following steps: The SBS resin is heated to 80-110° C., an acid catalyst and palm oil are added, and the mixture is kept warm to obtain a mixture; the mixture is subjected to high-speed shearing at 90-100° C. to obtain a palm oil-modified SBS resin.
[0010] More preferably, the insulation time is 1-2h.
[0011] Further preferably, the acidic catalyst is a 1-2 mol / L sulfuric acid solution.
[0012] Further preferably, the amount of the acidic catalyst added is 1%-5% of the mass of the SBS resin.
[0013] Further preferably, the amount of palm oil added is 10%-25% of the mass of the SBS resin.
[0014] Further preferably, the rotation speed of the high-speed shearing is 1800-2500 rpm, and the time of the high-speed shearing is 30-60 min.
[0015] Preferably, the method for preparing the palm fiber modified rubber particles comprises the following steps: S1, crushing the palm fiber, adding it into an alkaline solution, and soaking it to obtain pretreated palm fiber; S2, crushing the waste rubber, mixing it once at 100-140° C., adding an anti-aging agent and the pretreated palm fiber, heating it to 150-160° C. for secondary mixing to obtain a rubber mixture; S3, adding an accelerator and a vulcanizing agent to the rubber mixture for vulcanization, cooling, and granulating to obtain palm fiber modified rubber particles.
[0016] Further preferably, in S1, the alkaline solution is a 0.1-0.5 mol / L sodium hydroxide solution.
[0017] Further preferably, in S1, the immersion time is 30-40 min.
[0018] More preferably, in S2, the time of the first mixing is 3-5 min.
[0019] More preferably, in S2, the secondary mixing time is 3-5 min.
[0020] Further preferably, in S2, the amount of the anti-aging agent added is 4%-6% of the mass of the waste rubber.
[0021] Further preferably, in S3, the amount of the accelerator added is 1%-3% of the mass of the rubber compound.
[0022] Further preferably, in S3, the amount of the vulcanizing agent added is 1%-3% of the mass of the rubber compound.
[0023] Further preferably, in S2, the anti-aging agent is SP.
[0024] Further preferably, in S3, the accelerator is NS.
[0025] More preferably, in S3, the vulcanizing agent is sulfur.
[0026] Preferably, the particle size of the steel slag powder is 100-1000 μm.
[0027] Preferably, the particle size of the palm fiber modified rubber particles is 1-5 mm.
[0028] The second aspect of the present invention provides a method for preparing the green low-temperature resistant composite asphalt material, comprising the following steps: Step 1: Weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 165-180° C. to obtain a first asphalt component; Step 2: Add palm oil modified SBS resin and steel slag powder to the first asphalt component, mix well, and then heat-treat at 170-185° C. to obtain a second asphalt component; Step 3: Add palm fiber modified rubber particles to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
[0029] Preferably, in step 2, the heat preservation treatment time is 1-2h.
[0030] The third aspect of the present invention provides an application of the green low-temperature resistant composite asphalt material or the green low-temperature resistant composite asphalt material prepared by the preparation method of the green low-temperature resistant composite asphalt material in the development of highway pavement materials.
[0031] In summary, the present invention uses rock asphalt and matrix asphalt as main components, supplemented by palm oil modified SBS resin, steel slag powder and palm fiber modified rubber particles, to prepare a green low temperature resistant composite asphalt material. The green low temperature resistant composite asphalt material has simple ingredients, simple preparation process and excellent performance, which effectively solves the problem of poor low temperature resistance of asphalt pavement with rock asphalt as the main raw material in the prior art, and provides a more economical and environmentally friendly technical solution for highway pavement materials. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1 This embodiment provides a green low-temperature resistant composite asphalt material, which specifically includes the following contents: The green low-temperature resistant composite asphalt material comprises the following raw material components in percentage by weight: 25% rock asphalt, 35% base asphalt, 5% palm oil modified SBS resin, 10% steel slag powder and 25% palm fiber modified rubber particles.
[0034] The preparation method of the green low-temperature resistant composite asphalt material comprises the following steps: Step 1: weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 175° C. to obtain a first asphalt component; Step 2: Add palm oil modified SBS resin and steel slag powder to the first asphalt component, mix well, and heat-treat at 180° C. for 1.5 hours to obtain a second asphalt component; Step 3: Add palm fiber modified rubber particles to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
[0035] The method for preparing the palm oil modified SBS resin comprises the following steps: The SBS resin was heated to 100°C, and a sulfuric acid solution (1.5 mol / L) of 4% by weight of the SBS resin and palm oil of 15% by weight of the SBS resin were added, and the mixture was kept warm for 1 hour to obtain a mixture; the mixture was subjected to high-speed shearing at 95°C and a rotation speed of 2000 rpm for 50 minutes to obtain a palm oil-modified SBS resin.
[0036] The preparation method of the palm fiber modified rubber particles comprises the following steps: S1. Crush the palm fiber, add it into a 0.3 mol / L sodium hydroxide solution, and soak it for 35 min to obtain pretreated palm fiber; S2, crushing the waste rubber, mixing it once at 120° C. for 4 min, adding 5% of the weight of the waste rubber anti-aging agent SP and the pretreated palm fiber, heating it to 155° C. for secondary mixing for 4 min, and obtaining a rubber mixture; S3. Add 2% of the mass of the rubber mixture, accelerator NS, and 2% of the mass of the rubber mixture, sulfur, to the rubber mixture for vulcanization, cooling, and granulation to obtain palm fiber modified rubber particles with a particle size of 3 mm.
[0037] The particle size of the steel slag powder is 150 μm.
[0038] Example 2 This embodiment provides a green low-temperature resistant composite asphalt material, which specifically includes the following contents: The green low-temperature resistant composite asphalt material comprises the following raw material components in percentage by mass: 5% rock asphalt, 40% base asphalt, 10% palm oil modified SBS resin, 15% steel slag powder and 30% palm fiber modified rubber particles.
[0039] The preparation method of the green low-temperature resistant composite asphalt material comprises the following steps: Step 1: Weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 170° C. to obtain a first asphalt component; Step 2: Add palm oil modified SBS resin and steel slag powder to the first asphalt component, mix well, and heat-treat at 185° C. for 1 hour to obtain a second asphalt component; Step 3: Add palm fiber modified rubber particles to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
[0040] The method for preparing the palm oil modified SBS resin comprises the following steps: The SBS resin was heated to 100°C, and a sulfuric acid solution (1.5 mol / L) of 4% by weight of the SBS resin and palm oil of 15% by weight of the SBS resin were added, and the mixture was kept warm for 1 hour to obtain a mixture; the mixture was subjected to high-speed shearing at 95°C and a rotation speed of 2000 rpm for 50 minutes to obtain a palm oil-modified SBS resin.
[0041] The preparation method of the palm fiber modified rubber particles comprises the following steps: S1. Crush the palm fiber, add it into a 0.3 mol / L sodium hydroxide solution, and soak it for 35 min to obtain pretreated palm fiber; S2, crushing the waste rubber, mixing it once at 120° C. for 4 min, adding 5% of the weight of the waste rubber anti-aging agent SP and the pretreated palm fiber, heating it to 155° C. for secondary mixing for 4 min, and obtaining a rubber mixture; S3. Add 2% of the mass of the rubber mixture, accelerator NS, and 2% of the mass of the rubber mixture, sulfur, to the rubber mixture for vulcanization, cooling, and granulation to obtain palm fiber modified rubber particles with a particle size of 3 mm.
[0042] The particle size of the steel slag powder is 400 μm.
[0043] Example 3 This embodiment provides a green low-temperature resistant composite asphalt material, which specifically includes the following contents: The green low-temperature resistant composite asphalt material comprises the following raw material components in percentage by mass: 30% rock asphalt, 25% base asphalt, 15% palm oil modified SBS resin, 10% steel slag powder and 20% palm fiber modified rubber particles.
[0044] The preparation method of the green low-temperature resistant composite asphalt material comprises the following steps: Step 1: Weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 170° C. to obtain a first asphalt component; Step 2: Add palm oil modified SBS resin and steel slag powder to the first asphalt component, mix well, and heat-treat at 185° C. for 1.5 hours to obtain a second asphalt component; Step 3: Add palm fiber modified rubber particles to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
[0045] The method for preparing the palm oil modified SBS resin comprises the following steps: The SBS resin was heated to 100°C, and a sulfuric acid solution (1.5 mol / L) of 4% by weight of the SBS resin and palm oil of 15% by weight of the SBS resin were added, and the mixture was kept warm for 1 hour to obtain a mixture; the mixture was subjected to high-speed shearing at 95°C and a rotation speed of 2000 rpm for 50 minutes to obtain a palm oil-modified SBS resin.
[0046] The preparation method of the palm fiber modified rubber particles comprises the following steps: S1. Crush the palm fiber, add it into a 0.3 mol / L sodium hydroxide solution, and soak it for 35 min to obtain pretreated palm fiber; S2, crushing the waste rubber, mixing it once at 120° C. for 4 min, adding 5% of the weight of the waste rubber anti-aging agent SP and the pretreated palm fiber, heating it to 155° C. for secondary mixing for 4 min, and obtaining a rubber mixture; S3. Add 2% of the mass of the rubber mixture, accelerator NS, and 2% of the mass of the rubber mixture, sulfur, to the rubber mixture for vulcanization, cooling, and granulation to obtain palm fiber modified rubber particles with a particle size of 3 mm.
[0047] The particle size of the steel slag powder is 300 μm.
[0048] Comparative Example 1 This comparative example provides a green low-temperature resistant composite asphalt material, which is different from Example 1 in that the palm oil-modified SBS resin in the green low-temperature resistant composite asphalt material is replaced with an equal amount of SBS resin, specifically including the following contents: The green low-temperature resistant composite asphalt material comprises the following raw material components in percentage by weight: 25% rock asphalt, 35% base asphalt, 5% SBS resin, 10% steel slag powder and 25% palm fiber modified rubber particles.
[0049] The preparation method of the green low-temperature resistant composite asphalt material comprises the following steps: Step 1: weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 175° C. to obtain a first asphalt component; Step 2: Add SBS resin and steel slag powder to the first asphalt component, mix well, and heat-treat at 180° C. for 1.5 hours to obtain a second asphalt component; Step 3: Add palm fiber modified rubber particles to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
[0050] The preparation method of the palm fiber modified rubber particles comprises the following steps: S1. Crush the palm fiber, add it into a 0.3 mol / L sodium hydroxide solution, and soak it for 35 min to obtain pretreated palm fiber; S2, crushing the waste rubber, mixing it once at 120° C. for 4 min, adding 5% of the weight of the waste rubber anti-aging agent SP and the pretreated palm fiber, heating it to 155° C. for secondary mixing for 4 min, and obtaining a rubber mixture; S3. Add 2% of the mass of the rubber mixture, accelerator NS, and 2% of the mass of the rubber mixture, sulfur, to the rubber mixture for vulcanization, cooling, and granulation to obtain palm fiber modified rubber particles with a particle size of 3 mm.
[0051] The particle size of the steel slag powder is 150 μm.
[0052] Comparative Example 2 This comparative example provides a green low-temperature resistant composite asphalt material, which is different from Example 1 in that the palm fiber modified rubber particles are replaced with an equal amount of rubber powder, specifically including the following contents: The green low-temperature resistant composite asphalt material comprises the following raw material components in percentage by mass: 25% rock asphalt, 35% base asphalt, 5% palm oil modified SBS resin, 10% steel slag powder and 25% rubber powder.
[0053] The preparation method of the green low-temperature resistant composite asphalt material comprises the following steps: Step 1: weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 175° C. to obtain a first asphalt component; Step 2: Add palm oil modified SBS resin and steel slag powder to the first asphalt component, mix well, and heat-treat at 180° C. for 1.5 hours to obtain a second asphalt component; Step 3: Add rubber powder to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
[0054] The method for preparing the palm oil modified SBS resin comprises the following steps: The SBS resin was heated to 100°C, and a sulfuric acid solution (1.5 mol / L) of 4% by weight of the SBS resin and palm oil of 15% by weight of the SBS resin were added, and the mixture was kept warm for 1 hour to obtain a mixture; the mixture was subjected to high-speed shearing at 95°C and a rotation speed of 2000 rpm for 50 minutes to obtain a palm oil-modified SBS resin.
[0055] The particle size of the steel slag powder is 150 μm.
[0056] In order to further reflect the technical effect of the present invention, the present invention carried out relevant performance tests on the composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2, specifically including the following contents: "Technical Specifications for Asphalt Pavement Construction" (JTG F40-2004) stipulates that the composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2 shall be subjected to softening point test, dynamic stability test, low temperature crack resistance test and water stability test; the test results are shown in Table 1.
[0057] Table 1 Test results of composite asphalt materials obtained in Examples 1-3 and Comparative Examples 1-2
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A green low-temperature resistant composite asphalt material, characterized by: The raw material components include the following mass percentages: 5%-30% of rock asphalt, 25%-40% of base asphalt, 10%-15% of palm oil modified SBS resin, 10%-15% of steel slag powder and 20%-30% of palm fiber modified rubber particles.
2. The green low-temperature resistant composite asphalt material according to claim 1, characterized in that: The preparation method of the palm oil modified SBS resin comprises the following steps: The SBS resin is heated to 80-110° C., an acid catalyst and palm oil are added, and the mixture is kept warm to obtain a mixture; the mixture is subjected to high-speed shearing at 90-100° C. to obtain a palm oil-modified SBS resin.
3. The green low-temperature resistant composite asphalt material according to claim 2, characterized in that: The acidic catalyst is a 1-2 mol / L sulfuric acid solution; and / or The amount of the acidic catalyst added is 1%-5% of the mass of the SBS resin; and / or The amount of palm oil added is 10%-25% of the mass of the SBS resin.
4. The green low-temperature resistant composite asphalt material according to claim 2, characterized in that: The insulation time is 1-2h; and / or The rotation speed of the high-speed shearing is 1800-2500 rpm, and the time of the high-speed shearing is 30-60 min.
5. The green low-temperature resistant composite asphalt material according to claim 1, characterized in that: The preparation method of the palm fiber modified rubber particles comprises the following steps: S1, crushing the palm fiber, adding it into an alkaline solution, and soaking it to obtain pretreated palm fiber; S2, crushing the waste rubber, mixing it once at 100-140° C., adding an anti-aging agent and the pretreated palm fiber, heating it to 150-160° C. for secondary mixing to obtain a rubber mixture; S3, adding an accelerator and a vulcanizing agent to the rubber mixture for vulcanization, cooling, and granulating to obtain palm fiber modified rubber particles.
6. The green low-temperature resistant composite asphalt material according to claim 5, characterized in that: In S1, the alkaline solution is a 0.1-0.5 mol / L sodium hydroxide solution; and / or In S1, the immersion time is 30-40 min; and / or In S2, the time of the first mixing is 3-5 min; and / or In S2, the secondary mixing time is 3-5 min; and / or In S2, the amount of the anti-aging agent added is 4%-6% of the mass of the waste rubber.
7. The green low-temperature resistant composite asphalt material according to claim 5, characterized in that: In S3, the amount of the accelerator added is 1%-3% of the mass of the rubber compound; and / or In S3, the amount of the vulcanizing agent added is 1%-3% of the mass of the rubber compound.
8. The method for preparing a green low-temperature resistant composite asphalt material according to any one of claims 1 to 7, characterized in that: The steps include: Step 1: weigh each component according to the designed ratio, mix the rock asphalt and the matrix asphalt evenly, and melt them at 165-180° C. to obtain a first asphalt component; Step 2: Add palm oil modified SBS resin and steel slag powder to the first asphalt component, mix well, and then heat-treat at 170-185° C. to obtain a second asphalt component; Step 3: Add palm fiber modified rubber particles to the second asphalt component and mix them evenly to obtain a green low-temperature resistant composite asphalt material.
9. The method for preparing a green low-temperature resistant composite asphalt material according to claim 8, characterized in that: In step 2, the heat preservation treatment time is 1-2h.
10. Use of the green low-temperature resistant composite asphalt material as described in any one of claims 1 to 7 or the green low-temperature resistant composite asphalt material prepared by the preparation method of the green low-temperature resistant composite asphalt material as described in claim 8 or 9 in the development of highway pavement materials.