Fireproof flame-retardant shaving board and preparation method thereof
By using soybean meal adhesives, calcium carbonate and tannin acid components in particleboard, combined with composite flame retardants of zinc borate, aluminum hydroxide and magnesium oxide, the problem of insufficient fire resistance of traditional particleboards is solved. , achieving efficient flame retardant effect and mechanical performance improvement, ensuring the safety and environmental protection performance of particleboard.
Patent Information
- Application Number
- CN202411410436.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional particle board has shortcomings in its fire resistance, is flammable and releases formaldehyde during preparation and use, posing a potential threat to human health and the environment.
Adhesives with soybean meal adhesives, calcium carbonate and tannin acid, combined with composite flame retardant of zinc borate, aluminum hydroxide and magnesium oxide, and excellent flame retardant properties are prepared through hot pressing molding process. Mechanical properties of particle board.
It forms an effective flame retardant barrier, improves the flame resistance and mechanical properties of particle board, slows down the combustion speed, reduces the temperature of the material surface, enhances the stability and density of the carbon layer, and significantly improves the fire resistance and environmental friendliness.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of particle boards, and in particular to a fire-resistant and flame-retardant particle board and a preparation method thereof. Background Art
[0002] With the rapid development of the construction, furniture and interior decoration industries, the requirements for materials are increasing day by day, especially the fire resistance and environmental protection performance of materials have become the focus of attention. Due to the limitations of the material itself and the preparation process, traditional particleboard has certain deficiencies in fire resistance, and it is easy to release harmful gases such as formaldehyde during the preparation and use process, posing a potential threat to human health and the environment.
[0003] Traditional particleboard is mainly made of wood shavings and adhesives, and its fireproof performance is limited by the flammability of the wood itself and the flame retardancy of the adhesive. In a fire, traditional particleboard tends to burn quickly, which is not conducive to fire control and personnel safety. At present, most particleboards are bonded with adhesives containing formaldehyde, resulting in a high amount of formaldehyde release during the preparation and use process, and long-term contact may cause harm to human health. In addition, the formaldehyde release cycle is long, and it may even remain in the building for several years, increasing the risk of environmental pollution. Based on this, the present invention proposes a fire-retardant particleboard and a preparation method thereof. Summary of the invention
[0004] The present invention provides a fire-retardant particleboard and a preparation method thereof, and prepares a particleboard with excellent flame retardant properties and mechanical properties. The components of the adhesive used, such as soybean meal adhesive, calcium carbonate and tannic acid, can synergistically act during the combustion process to form an effective flame retardant barrier; at the same time, they can also improve the mechanical properties of the particleboard through mechanisms such as bonding, filling and reinforcement.
[0005] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a fireproof and flame-retardant particleboard, comprising the following raw materials in parts by weight: 14-18 parts of wood particles, 0.25-0.35 parts of adhesive, and 1-1.4 parts of flame retardant; the moisture content of the particleboard is 6%-8%.
[0006] As a further technical solution, the wood shavings are poplar wood shavings that are baked and dried to a moisture content of no more than 3%; the wood shavings have a length of 10-12 mm, a width of 5-6 mm, and a thickness of 0.2-0.3 mm.
[0007] As a further technical solution, the preparation method of the adhesive includes: taking water and soybean meal, mixing and stirring for 15-25 minutes to form a homogeneous system, and obtaining soybean meal adhesive; taking calcium carbonate and ultrasonically cleaning it for 30-40 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 10%-12%, heating it to 85-95°C until the polyvinyl alcohol is completely dissolved, cooling it to 60-70°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate, mixing them evenly to obtain a mixture, adding a tannic acid solution, and centrifuging to remove the supernatant to obtain an adhesive.
[0008] As a further technical solution, the weight ratio of water to soybean meal is (35-40): (12-16), wherein the protein content of soybean meal is 44%-48%.
[0009] As a further technical solution, the weight ratio of the polyvinyl alcohol aqueous solution, soybean meal adhesive and ultrasonically treated calcium carbonate is 1:(1-2):(1-2).
[0010] As a further technical solution, the centrifugal speed is 2200-2600r / min, and the centrifugal time is 30-40min.
[0011] As a further technical solution, the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 10%-12%, and the mass of the tannic acid solution is 40%-50% of the mass of the polyvinyl alcohol aqueous solution. As a further technical solution, the flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of (4-5): (0.2-0.4): (1-2).
[0012] Among them, zinc borate will decompose at high temperature and release crystal water. When these water evaporates, they will absorb a lot of heat, thereby reducing the temperature of the material surface and slowing down the combustion rate. At the same time, the borate generated after the decomposition of zinc borate covers the surface of the material, forming a protective layer, isolating oxygen and combustible gases, and further inhibiting combustion. In addition, the boron element can also promote the formation of the carbon layer, enhance the stability and density of the carbon layer, and improve the material's anti-ablation ability. The flame retardant principle of aluminum hydroxide mainly includes two aspects: heat absorption and cooling and dehydration film formation. During the combustion process, aluminum hydroxide will decompose to generate water and absorb a lot of heat, thereby reducing the temperature of the material surface and slowing down the combustion rate. At the same time, the decomposed aluminum oxide covers the surface of the material, forming a dense protective film, isolating oxygen and combustible gases, and inhibiting the combustion. In addition, aluminum oxide also has a high melting point and can maintain stability at high temperatures, further enhancing the flame retardant properties of the material. During the combustion process, magnesium oxide can form a hard protective layer that covers the surface of the material, isolating oxygen and combustible gases, thereby inhibiting the combustion. In addition, magnesium oxide has high thermal and chemical stability, can maintain the stability of its structure and performance at high temperatures, and is not easily destroyed by combustion.
[0013] In a second aspect, the present invention proposes a method for preparing a fireproof and flame-retardant particleboard, the steps comprising: mixing the raw materials of the flame retardant evenly to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, standing at room temperature for 5-6 days after cooling, and trimming and sanding the hot-pressed plate blank to obtain the obtained material.
[0014] As a further technical solution, the hot pressing molding temperature is 160-170°C, the hot pressing pressure is 1.5MPa-2.5MPa, and the hot pressing time is 4-5min.
[0015] The working principle and beneficial effects of the present invention are: 1. The adhesive of the present invention can effectively improve the adhesion between particle materials, and improve the mechanical properties of particleboard through bonding, filling and reinforcement mechanisms; at the same time, the components such as soybean meal adhesive, calcium carbonate and tannic acid in the adhesive can work synergistically during the combustion process to form an effective flame retardant barrier.
[0016] 2. The protein and carbohydrates in the soybean meal adhesive can form a network structure during the stirring and curing process. This structure can firmly bond the wood particles together to form a board with high overall strength. The soybean meal adhesive also has a certain elasticity, which can absorb and disperse external impact and improve the anti-destruction ability of the particleboard. Calcium carbonate, as an inorganic filler, can fill the gaps between the wood particles, reduce the porosity inside the board, and improve the density and hardness. The addition of calcium carbonate can also improve the dimensional stability of the board and reduce the expansion and contraction caused by humidity changes. Polyvinyl alcohol, as a water-soluble polymer material, has good adhesion and film-forming properties. In the adhesive, it can act as a binder to firmly combine the soybean meal adhesive, calcium carbonate and other components together; the addition of polyvinyl alcohol can also improve the water resistance and weather resistance of the adhesive, so that the particleboard can still maintain good mechanical properties in a humid or harsh environment.
[0017] 3. The adhesive in the present invention also has a certain flame retardant effect. As a natural polymer material, soybean meal is rich in protein and carbohydrates. During the combustion process, these components can form a dense carbon layer, which effectively isolates the transfer of oxygen and heat, thereby slowing down the combustion rate. Calcium carbonate will decompose at high temperatures to produce carbon dioxide and water vapor. These gases can dilute the concentration of combustible gases and oxygen, reduce the temperature and flame propagation speed of the combustion area; and the solid residues produced by decomposition (such as calcium oxide) can increase the thickness and stability of the carbon layer, forming a more effective thermal insulation barrier. The added tannic acid, as a polyphenol compound, has excellent thermal stability and antioxidant properties. During the combustion process, it can react chemically with the components in the soybean meal to generate a more stable carbon layer structure; in addition, tannic acid can also react with the alkaline substances produced by the decomposition of calcium carbonate to form compounds with higher flame retardant properties.
[0018] 4. The present invention also adds a compound flame retardant of zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of (4-5): (0.2-0.4): (1-2). When the three flame retardants are compounded, they will produce a synergistic effect, further improving the flame retardant effect. Specifically, these three flame retardants each exert their unique flame retardant mechanism during the combustion process, while complementing and enhancing each other. Among them, zinc borate and aluminum hydroxide can form a protective layer to isolate oxygen and combustible gases, but the protective layers they form are different in composition and structure. After compounding, a more stable and dense protective layer can be formed; magnesium oxide can enhance the hardness and high temperature resistance of the protective layer, further improving the flame retardant properties of the material. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1 The present embodiment provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0021] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1.5:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 4.5:0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0022] Example 2 The present embodiment provides a fireproof and flame-retardant particle board, which is composed of the following raw materials in parts by weight: 14 parts of particle board, 0.25 parts of adhesive, and 1 part of flame retardant; the moisture content of the particle board is 6%; the particle board is poplar particle board that has been dried to a moisture content of 3%; the particle board has a length of 10 mm, a width of 5 mm, and a thickness of 0.2 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0023] The preparation method of the adhesive includes: mixing water and soybean meal for 15 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 30 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 10%, heating it to 85°C until the polyvinyl alcohol is completely dissolved, cooling it to 60°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 10%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 35:12, wherein the protein content of soybean meal is 44%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1:1; the centrifugal speed is 2200r / min, and the centrifugal time is 30min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 10%, and the mass of the tannic acid solution is 40% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 4:0.2:1; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the shavings and the adhesive, placing the mixed material in a mold for hot pressing molding, wherein the hot pressing molding temperature is 160°C, the hot pressing pressure is 1.5MPa, and the hot pressing time is 4min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing molded plate blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0024] Example 3 The present embodiment provides a fireproof and flame-retardant particle board, which is composed of the following raw materials in parts by weight: 18 parts of particle board, 0.35 parts of adhesive, and 1.4 parts of flame retardant; the moisture content of the particle board is 8%; the particle board is poplar particle board that has been dried to a moisture content of 3%; the particle board has a length of 12 mm, a width of 6 mm, and a thickness of 0.3 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0025] The preparation method of the adhesive includes: mixing water and soybean meal for 25 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 40 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 12%, heating it to 95°C until the polyvinyl alcohol is completely dissolved, cooling it to 70°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 12%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 40:16, wherein the protein content of soybean meal is 48%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:2:2; the centrifugal speed is 2600r / min, and the centrifugal time is 40min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 12%, and the mass of the tannic acid solution is 50% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 5:0.4:2; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the shavings and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 170°C, the hot pressing pressure is 2.5MPa, and the hot pressing time is 5min. After cooling, the mixture is allowed to stand at room temperature for 6 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0026] Example 4 The present embodiment provides a fireproof and flame-retardant particle board, which is composed of the following raw materials in parts by weight: 14 parts of particle board, 0.35 parts of adhesive, and 1 part of flame retardant; the moisture content of the particle board is 8%; the particle board is poplar particle board that has been dried to a moisture content of 3%; the particle board has a length of 10 mm, a width of 6 mm, and a thickness of 0.2 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0027] The preparation method of the adhesive includes: mixing water and soybean meal for 25 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 30 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 12%, heating it to 85°C until the polyvinyl alcohol is completely dissolved, cooling it to 70°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 10%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 40:12, wherein the protein content of soybean meal is 44%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:2:1; the centrifugal speed is 2600r / min, and the centrifugal time is 30min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 12%, and the mass of the tannic acid solution is 40% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 5:0.2:2; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 160°C, the hot pressing pressure is 2.5MPa, and the hot pressing time is 4min. After cooling, the mixture is allowed to stand at room temperature for 6 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0028] Comparative Example 1 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0029] The preparation method of the adhesive comprises: taking calcium carbonate and performing ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the ultrasonically treated calcium carbonate and mixing it evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain the adhesive; the weight ratio of the polyvinyl alcohol aqueous solution to the ultrasonically treated calcium carbonate is 1:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35 minutes; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 4.5:0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0030] Comparative Example 2 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0031] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain a soybean meal adhesive; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and mixing it evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution to the soybean meal adhesive is 1:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 4.5:0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0032] Comparative Example 3 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0033] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, and centrifuging to remove the supernatant to obtain the adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1.5:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 4.5:0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0034] Comparative Example 4 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0035] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 2:1:1; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of 4.5:0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0036] Comparative Example 5 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0037] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1.5:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes aluminum hydroxide and magnesium oxide in a weight ratio of 0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0038] Comparative Example 6 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0039] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1.5:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate and magnesium oxide in a weight ratio of 4.5:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0040] Comparative Example 7 The present comparative example provides a fireproof and flame-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of particleboard, 0.3 parts of adhesive, and 1.2 parts of flame retardant; the moisture content of the particleboard is 7%; the particleboard is poplar particleboard that has been dried to a moisture content of 3%; the particleboard has a length of 11 mm, a width of 5.5 mm, and a thickness of 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0041] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1.5:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The flame retardant includes zinc borate and aluminum hydroxide in a weight ratio of 0.3:1.5; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2 MPa, and the hot pressing time is 4.5 minutes; after cooling, standing at room temperature for 5 days; trimming and sanding the hot pressing plate blank to obtain the fireproof and flame-retardant particleboard.
[0042] Comparative Example 8 The present comparative example provides a fire-retardant particleboard, which is composed of the following raw materials in parts by weight: 16 parts of wood particles, 0.3 parts of adhesive, and the moisture content of the particleboard is 7%; the wood particles are poplar wood particles that are dried to a moisture content of 3%; the length of the wood particles is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; In other embodiments, auxiliary agents such as waterproofing, mildew-proofing, and sterilization may also be added.
[0043] The preparation method of the adhesive includes: mixing water and soybean meal for 20 minutes to form a homogenous system to obtain soybean meal adhesive; taking calcium carbonate for ultrasonic cleaning for 35 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 11%, heating it to 90°C until the polyvinyl alcohol is completely dissolved, cooling it to 65°C, adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to mix evenly to obtain a mixture, adding a tannic acid aqueous solution with a mass fraction of 11%, and centrifuging to remove the supernatant to obtain an adhesive; the weight ratio of water to soybean meal is 37:14, wherein the protein content of soybean meal is 46%; the weight ratio of the polyvinyl alcohol aqueous solution, the soybean meal adhesive and the ultrasonically treated calcium carbonate is 1:1.5:1.5; the centrifugal speed is 2400r / min, and the centrifugal time is 35min; the tannic acid solution is a tannic acid aqueous solution with a mass fraction of 11%, and the mass of the tannic acid solution is 45% of the mass of the polyvinyl alcohol aqueous solution; The preparation method of the fireproof and flame-retardant particleboard comprises the following steps: uniformly mixing raw materials of the flame retardant to obtain the flame retardant, stirring and mixing with the wood chips and the adhesive, placing the mixed material in a mold for hot pressing, wherein the hot pressing temperature is 165°C, the hot pressing pressure is 2MPa, and the hot pressing time is 4.5min. After cooling, the mixture is allowed to stand at room temperature for 5 days, and the hot pressing blank is trimmed and sanded to obtain the fireproof and flame-retardant particleboard.
[0044] Test Example 1: The fire-retardant particleboards (with a thickness of 10 mm and a width of 300 mm×300 mm×10 mm) prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-8 were tested as follows: Mechanical properties: The mechanical properties of particleboard were tested according to GB / T4897-2015 "Particleboard" standard; Combustion performance: The limiting oxygen index is tested according to standard GB / T2406.2-2009; The results are shown in Table 1 below: Table 1
[0045] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A fire-retardant particleboard, characterized in that: The invention comprises the following raw materials in parts by weight: 14-18 parts of wood chips, 0.25-0.35 parts of adhesive, and 1-1.4 parts of flame retardant; the moisture content of the particle board is 6%-8%.
2. The fire-retardant particle board according to claim 1, characterized in that: The wood shavings are poplar wood shavings that are baked and dried to a moisture content of no more than 3%; the wood shavings have a length of 10-12 mm, a width of 5-6 mm, and a thickness of 0.2-0.3 mm.
3. The fire-retardant particleboard according to claim 1, characterized in that: The preparation method of the adhesive comprises: mixing water and soybean meal for 15-25 minutes to form a homogenous system to obtain soybean meal adhesive; ultrasonic cleaning of calcium carbonate for 30-40 minutes; preparing a polyvinyl alcohol aqueous solution with a mass fraction of 10%-12%, heating it to 85-95° C. until the polyvinyl alcohol is completely dissolved, cooling it to 60-70° C., adding the soybean meal adhesive and the ultrasonically treated calcium carbonate to obtain a mixture after mixing evenly, adding a tannic acid solution, and centrifuging to remove the supernatant to obtain an adhesive.
4. The fire-retardant particle board according to claim 3, characterized in that: The weight ratio of water to soybean meal is (35-40): (12-16), wherein the protein content of soybean meal is 44%-48%.
5. The fire-retardant particle board according to claim 3, characterized in that: The weight ratio of the polyvinyl alcohol aqueous solution, soybean meal adhesive and ultrasonically treated calcium carbonate is 1:(1-2):(1-2).
6. The fire-retardant particle board according to claim 3, characterized in that: The centrifugal speed is 2200-2600 r / min, and the centrifugal time is 30-40 min.
7. The fire-retardant particle board according to claim 3, characterized in that: The tannic acid solution is a tannic acid aqueous solution with a mass fraction of 10%-12%, and the mass of the tannic acid solution is 40%-50% of the mass of the polyvinyl alcohol aqueous solution.
8. The fire-retardant particle board according to claim 1, characterized in that: The flame retardant comprises zinc borate, aluminum hydroxide and magnesium oxide in a weight ratio of (4-5): (0.2-0.4): (1-2).
9. A method for preparing a fire-retardant particleboard according to any one of claims 1 to 8, characterized in that the steps include: The raw materials of the flame retardant are uniformly mixed to obtain the flame retardant, and the mixture is stirred and mixed with the wood chips and the adhesive, and the mixture is placed in a mold for hot pressing and formed, and after cooling, it is allowed to stand at room temperature for 5-6 days, and the hot pressing formed plate blank is trimmed and sanded to obtain the flame retardant.
10. The method for preparing a fire-retardant particleboard according to claim 9, characterized in that: The hot pressing molding temperature is 160-170° C., the hot pressing pressure is 1.5 MPa-2.5 MPa, and the hot pressing time is 4-5 min.