Marine light low-toxicity flame-retardant putty and preparation method thereof

By using a combination formula of VAE emulsion, phosphorus-nitrogen-based flame retardant and light filler in flame retardant putty, the density increase and performance reduction caused by the improvement of flame retardant performance in the prior art is solved, and high solids content and low The marine lightweight, low-toxic flame retardant putty with density and high bonding strength meets the fireproof needs of ships.

CN119081462AInactive Publication Date: 2024-12-06WUHAN INSTITUTE OF MARINE ELECTRIC PROPULSION (THE 712TH RESEARCH INSTITUTE OF CHINA STATE SHIPBUILDING CORP LTD)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411467388.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When existing flame retardant putty improves flame retardant performance, it will reduce conventional performance, easily age, powder, low peel strength, sharp increase in density, increase the weight of the ship, and it is difficult to meet the flame retardant, bonding strength and low water absorption rate at the same time. Require.

Method used

Lightweight, low-toxic flame retardant putty formula with aqueous ethylene-vinyl acetate copolymer (VAE) emulsion as the base, combined with phosphorus-nitrogen flame retardant, aluminum hydroxide, lightweight calcium carbonate, closed-cell hollow microbeads and aerogels , through grinding, high-speed stirring and compounding, a high-solid content paste is prepared to ensure flame retardancy and bonding strength while reducing density.

Benefits of technology

It realizes the effective reduction of flame retardant putty density while ensuring flame retardant strength, and meets the needs of ship weight reduction and energy saving and emission reduction. The density is <1.3g/cm3, the ultimate oxygen index ≥30, and the peel strength at room temperature ≥3N/cm, comply with the "2010 FTP Rules" and the national tobacco toxicity standards.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses light low-toxicity flame-retardant putty for ships. The putty is prepared from 40-60 parts of VAE emulsion, 20-40 parts of a phosphorus-nitrogen flame retardant, 2-16 parts of a dispersing agent, 10-20 parts of aluminum hydroxide, 30-50 parts of light calcium carbonate, 10-15 parts of closed-cell hollow microspheres, 5-10 parts of aerogel, 1-5.5 parts of a thickening agent, 1 part of 2, 2, 4-trimethyl-1, 3-pentanediol monoisobutyrate and 1 part of distilled water. The mesh number of the aluminum hydroxide and the light calcium carbonate is more than 2000; the closed pore type hollow microspheres are borosilicate with the mesh number of more than 2000 meshes, the wall thickness of 1-2 microns and the aperture ratio of less than 5%; the invention further discloses a preparation method. On the premise of not reducing the peel strength, by optimizing the formula of the solid filler, reducing the density of the adhesive, reducing the weight of a ship body and increasing the water resistance, the flame-retardant and safety performance requirements are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of marine putty, and particularly relates to a marine light-weight, low-toxic flame-retardant putty, and a preparation method thereof. Background Art

[0002] Flame retardant putty is one of the most commonly used engineering materials. Although it has certain flame retardant properties, the flame retardant mechanism is mainly based on the gas phase flame retardant mechanism and does not have the effect of carbonization. However, in order to pass the BS-5852:2006 flame retardant test standard, flame retardant putty alone will be added with flame retardants. The product improves the flame retardant performance while reducing the conventional performance. After construction, it is easy to age, powder, and have low peel strength. The density will increase sharply, generally at 2.5g / cm 3 The above greatly increases the weight of the ship. Summary of the invention

[0003] In order to overcome the above technical problems in the prior art, one of the purposes of the present invention is to provide a lightweight, flame retardant, non-toxic water-based ethylene-vinyl acetate copolymer (VAE emulsion) adhesive as a base flame retardant putty.

[0004] The technical solution adopted by the present invention to solve the technical problem is: a light and low-toxic flame-retardant putty for ships, wherein the components of the formula include 40-60 parts of VAE emulsion, 15-43 parts of phosphorus-nitrogen flame retardant, 2-16 parts of dispersant, 10-20 parts of aluminum hydroxide, 30-50 parts of light calcium carbonate, 10-15 parts of closed-cell hollow microspheres, 5-10 parts of aerogel, 1-5.5 parts of thickener, 1 part of film-forming aid dodecyl alcohol ester and 1 part of distilled water; the mesh numbers of the aluminum hydroxide and the light calcium carbonate are above 2000 meshes; the closed-cell hollow microspheres are borosilicates with a mesh number of above 2000 meshes, a wall thickness of 1-2 μm and an opening rate of less than 5%.

[0005] Furthermore, the phosphorus-nitrogen flame retardant is a combination of two or more of ammonium polyphosphate, melamine pyrophosphate, melamine, and zinc oxide.

[0006] Furthermore, the dispersant is a combination of two or more of sodium polyacrylate, sodium tripolyphosphate, polyoxyethylene fatty acid ester, sodium lauryl sulfate, and pentaerythritol.

[0007] Furthermore, the thickener is aqueous thickener TT935 or carboxymethyl cellulose.

[0008] The second object of the present invention is to provide a method for preparing a lightweight and low-toxic flame-retardant putty for ships, the steps of which are as follows: (1) First, a phosphorus-nitrogen flame retardant, a dispersant, aluminum hydroxide and distilled water are added to a reactor for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid with a certain solid content; (2) Adding VAE emulsion into a stirrer, compounding the flame retardant liquid and VAE emulsion, stirring at high speed, and dispersing the system until the latex particle diameter is less than 10 μm, thereby obtaining a flame retardant emulsion; (3) Adding filler light calcium carbonate, closed-cell hollow microspheres, aerogel, thickener and film-forming aid to the flame-retardant emulsion of step (2), and stirring thoroughly to obtain a light and low-toxic flame-retardant putty.

[0009] The beneficial effects of the present invention are: The present invention adds and optimizes the ratio of light calcium carbonate, closed-cell hollow microspheres and aerogel on the basis of conventional VAE emulsions available on the market, thereby effectively reducing the density of the flame retardant putty while ensuring flame retardancy, bonding strength and increasing solid content. At the same time, by screening lightweight fillers, the stability of the mixed system is guaranteed, and demulsification, precipitation, phase separation and other deterioration conditions will not occur. At the same time, the flame retardant is pre-dispersed, and the composition of the flame retardant, the ratio of the flame retardant liquid and the emulsion are adjusted to prepare coating adhesives that meet customer requirements for different flame retardant levels. At the same time, this product uses inorganic flame retardants and flame retardant synergists in appropriate proportions as the flame retardant system, which can not only isolate oxygen and heat on the surface of the glued building, but also have a smoke suppression effect; The present invention innovatively uses three kinds of lightweight fillers in combination, which effectively reduces the density of flame-retardant putty with high solid content while meeting the requirements of bonding strength, flame retardancy and low water absorption, laying a good foundation for ship weight reduction, energy conservation and emission reduction. The flame retardant putty of the present invention has a higher solid content (>75%) and is a paste-like substance compared with conventional putty powder, and can be directly used for construction without adding water for further processing; The basic parameters of the lightweight and low-toxic flame-retardant putty prepared in the present invention meet the following requirements: density <1.3 g / cm 3 , limiting oxygen index ≥30, room temperature peel strength ≥3N / cm, non-volatile content 80-90%, actual drying time ≤12h, storage stability ≥12 months. Safety performance meets the performance requirements for bulkheads, linings or ceilings in Part 2 and Part 5 of Annex 1 of the 2010 FTP Rules. Smoke toxicity meets the identification standards of relevant national institutions. DETAILED DESCRIPTION

[0010] The present invention will be further described below in conjunction with specific embodiments. Example 1

[0011] This embodiment discloses a light-weight, low-toxic flame-retardant putty for ships, and the preparation steps are as follows.

[0012] First, add 10 parts of ammonium polyphosphate, 5 parts of melamine pyrophosphate, 5 parts of zinc oxide, 1 part of sodium tripolyphosphate, 1 part of polyoxyethylene fatty acid ester, 10 parts of aluminum hydroxide and 1 part of distilled water into a disperser for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid with a certain solid content; add 40 parts of VAE emulsion into the stirrer, compound the flame retardant liquid and VAE emulsion, stir at high speed and disperse until the system is uniform, so that the diameter of the latex particles is less than 10μm; finally, add 30 parts of light calcium carbonate, 15 parts of borosilicate, 5 parts of aerogel, 2 parts of water-based thickener TT935 to the flame retardant emulsion to achieve thickening effect and 1 part of dodecyl alcohol ester to help film formation, stir thoroughly and filter to obtain a water-based flame retardant putty. Example 2

[0013] This embodiment discloses a light-weight, low-toxic flame-retardant putty for ships, and the preparation steps are as follows.

[0014] First, add 20 parts of ammonium polyphosphate, 7.5 parts of melamine, 12.5 parts of zinc oxide, 10 parts of pentaerythritol, 3 parts of sodium polyacrylate, 3 parts of sodium lauryl sulfate, 15 parts of aluminum hydroxide and 1 part of distilled water into a disperser for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid with a certain solid content; add 60 parts of VAE emulsion into the stirrer, compound the flame retardant liquid and VAE emulsion, stir at high speed and disperse until the system is uniform, so that the diameter of the latex particles is less than 10μm; finally, add 35 parts of light calcium carbonate, 12 parts of borosilicate, 10 parts of aerogel, 5.5 parts of carboxymethyl cellulose to the flame retardant emulsion to achieve thickening effect and 1 part of dodecyl alcohol ester to help film formation, stir thoroughly to obtain a water-based flame retardant putty. Example 3

[0015] This embodiment discloses a light-weight, low-toxic flame-retardant putty for ships, and the preparation steps are as follows.

[0016] First, add 10 parts of ammonium polyphosphate, 15 parts of melamine pyrophosphate, 1 part of sodium tripolyphosphate, 1 part of polyoxyethylene fatty acid ester, 10 parts of aluminum hydroxide and 1 part of distilled water into a disperser for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid with a certain solid content; add 55 parts of VAE emulsion into the stirrer, compound the flame retardant liquid and VAE emulsion, stir at high speed and disperse until the system is uniform, so that the diameter of the latex particles is less than 10μm; finally, add 40 parts of light calcium carbonate, 10 parts of borosilicate, 8 parts of aerogel, 1 part of water-based thickener TT935 to the flame retardant emulsion to achieve thickening effect and 1 part of dodecyl alcohol ester to help film formation, stir thoroughly and filter to obtain a water-based flame retardant putty. Example 4

[0017] This embodiment discloses a light-weight, low-toxic flame-retardant putty for ships, and the preparation steps are as follows.

[0018] First, add 5 parts of ammonium polyphosphate, 10 parts of melamine pyrophosphate, 5 parts of zinc oxide, 1 part of sodium tripolyphosphate, 4 parts of polyoxyethylene fatty acid ester, 10 parts of aluminum hydroxide and 1 part of distilled water into a disperser for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid with a certain solid content; add 50 parts of VAE emulsion into the stirrer, compound the flame retardant liquid and VAE emulsion, stir at high speed and disperse until the system is uniform, so that the diameter of the latex particles is less than 10μm; finally, add 40 parts of light calcium carbonate, 10 parts of borosilicate, 5 parts of aerogel, 3 parts of water-based thickener TT935 to the flame retardant emulsion to achieve thickening effect and 1 part of dodecyl alcohol ester to help film formation, stir thoroughly and filter to obtain a water-based flame retardant putty. Example 5

[0019] This embodiment discloses a light-weight, low-toxic flame-retardant putty for ships, and the preparation steps are as follows.

[0020] First, add 15 parts of ammonium polyphosphate, 10 parts of melamine, 12.5 parts of zinc oxide, 10 parts of pentaerythritol, 2 parts of sodium polyacrylate, 3 parts of sodium lauryl sulfate, 20 parts of aluminum hydroxide and 1 part of distilled water into a disperser for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid with a certain solid content; add 45 parts of VAE emulsion into the stirrer, compound the flame retardant liquid and VAE emulsion, stir at high speed and disperse until the system is uniform, so that the diameter of the latex particles is less than 10μm; finally, add 50 parts of light calcium carbonate, 10 parts of borosilicate, 10 parts of aerogel, 5.5 parts of carboxymethyl cellulose to the flame retardant emulsion to achieve thickening effect and 1 part of dodecyl alcohol ester to help film formation, stir thoroughly to obtain a water-based flame retardant putty.

[0021] Since the paste putty requires a solid content of more than 75%, the increase in solid content will reduce the bonding strength of the water-based putty, while greatly increasing the density, increasing the weight of the ship, and thus increasing energy consumption. The lightweight, low-toxic flame-retardant putty prepared by the present invention is mainly used for leveling fireproof panels in the shipbuilding process. It is a single-component water-based paste, not putty powder. The adhesive performance test results are shown in the following table.

[0022] .

[0023] The above embodiments are only intended to illustrate the technical solutions of the present invention, rather than all embodiments. Any modifications, equivalent substitutions and improvements made within the principles of the present invention are all within the protection scope of the present invention.

Claims

1. A lightweight and low-toxic flame-retardant putty for ships, characterized in that: It includes 40-60 parts of VAE emulsion, 15-43 parts of phosphorus-nitrogen flame retardant, 2-16 parts of dispersant, 10-20 parts of aluminum hydroxide, 30-50 parts of light calcium carbonate, 10-15 parts of closed-cell hollow microspheres, 5-10 parts of aerogel, 1-5.5 parts of thickener, 1 part of dodecyl alcohol ester and 1 part of distilled water; the mesh size of the aluminum hydroxide and light calcium carbonate is more than 2000 mesh; the closed-cell hollow microspheres are borosilicate with a mesh size of more than 2000 mesh, a wall thickness of 1-2μm and an opening rate of less than 5%.

2. A lightweight and low-toxic flame-retardant putty for ships according to claim 1, characterized in that: The phosphorus-nitrogen flame retardant is a combination of two or more of ammonium polyphosphate, melamine pyrophosphate, melamine and zinc oxide.

3. A light and low-toxic flame-retardant putty for ships according to claim 1 or 2, characterized in that: The dispersant is a combination of two or more of sodium polyacrylate, sodium tripolyphosphate, polyoxyethylene fatty acid ester, sodium lauryl sulfate and pentaerythritol.

4. A light and low-toxic flame-retardant putty for ships according to claim 3, characterized in that: The thickener is water-based thickener TT935 or carboxymethyl cellulose.

5. A method for preparing the lightweight and low-toxic flame-retardant putty for ships as claimed in claim 1, characterized in that: Here are the steps: (1) Adding a phosphorus-nitrogen flame retardant, a dispersant, aluminum hydroxide and distilled water into a reactor for grinding, high-speed stirring and dispersion to prepare a flame retardant liquid; (2) Adding VAE emulsion into a stirrer, compounding the flame retardant liquid and the VAE emulsion and stirring at a high speed so that the diameter of the latex particles is less than 10 μm, thereby obtaining a flame retardant emulsion; (3) Light calcium carbonate, closed-cell hollow microspheres, aerogel, thickener and film-forming aid are added to the flame retardant emulsion and stirred thoroughly to obtain a light and low-toxic flame retardant putty for ships.

Citation Information

Patent Citations

  • High-temperature aerogel heat-insulation fireproof coating and preparation method thereof

    CN112500770A

  • Intrinsic hydrophobic non-intumescent fire retardant coating material for steel structure

    CN112876889A

  • Two-component multifunctional waterproof heat-insulation putty and use method thereof

    CN113667345A